A conductive polylactic acid composite material and preparation method thereof

The in situ reduction reaction of the polylactic acid material is used to form surface-loaded nano zinc oxide, copper/silver particles by using graphene oxide modified with silane coupling agent in polylactic acid material, and combined with carbonyl addition reaction, the uneven conductivity of polylactic acid material is solved. The problem is that high conductivity and strong bonding strength are achieved, and the application range of melt deposition molding processes is expanded.

CN116082810BActive Publication Date: 2024-11-22HUAIYIN INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211631154.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-11-22
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

When the prior art, when fibers and particulate fillers are added to polylactic acid materials to enhance performance and impart conductive functions, the mixture phase is uneven due to differences in physical properties of the material during the molding process, the bonding strength is insufficient, the conductivity is uneven and difficult to control.

Method used

Graphene oxide with halogenated alkane branched chain modified by silane coupling agent is used to form graphene oxide with surface-loaded nano zinc oxide and copper/silver particles through in-situ reduction reaction, and carbonyl addition reaction is carried out with polylactic acid. Enhance the bonding strength and conductivity, and perform precision molding in combination with the melt deposition molding process.

Benefits of technology

It significantly improves the conductive function of polylactic acid materials and the conductivity of molded parts, provides special conductive raw materials, broadens the types and methods of raw materials for the melt deposition molding process, and realizes the precision manufacturing of complex structure conductive functional devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116082810B_ABST
    Figure CN116082810B_ABST
Patent Text Reader

Abstract

The invention discloses a conductive polylactic acid composite material and a preparation method thereof. The raw materials of the conductive polylactic acid composite material include polylactic acid and graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface. The preparation method is as follows: firstly prepare graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface, then add the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles, then add the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and then add the graphene oxide to liquid polylactic acid, stir and mix, and then perform extrusion, water condensation, solidification and melt deposition molding to obtain the conductive polylactic acid composite material. The invention adopts nano Zn to perform in-situ reduction reaction on graphene oxide with halogenated alkane side chains modified by a silane coupling agent, copper ions and silver ions, and then utilizes the addition reaction between graphene oxide with halogenated alkane side chains modified by a silane coupling agent and carbonyl groups of polylactic acid to form a strong chemical bond, so as to obtain the polylactic acid composite material with excellent conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a conductive material and a preparation method thereof, and in particular to a conductive polylactic acid composite material and a preparation method thereof. Background Art

[0002] With the rapid development of society, people's demand for functional products is increasing, especially polymer products with new conductive functions, such as wearable sensor electronic devices, shape memory devices and other conductive functional components. The fused deposition modeling process provides technical support for the manufacture of complex structure functional polymer devices, but due to the lack of corresponding special conductive raw materials, it is difficult to directly give the above components conductive functions. Therefore, the fused deposition modeling functional components have become a scientific and technological problem that needs to be solved in this field. At present, the existing technology mainly attempts to add different fibers and particle fillers to polylactic acid to enhance the performance of polylactic acid materials or develop new functions. For example, a composite material of carbon nanotubes, polylactic acid and silicone elastomer is obtained as a functional raw material by mechanical mixing. However, due to the difference in material properties during the molding process, it is difficult to effectively ensure the uniformity and bonding strength of each mixed phase due to the mechanically mixed composite material, resulting in uneven conductivity and different performance of the molded parts, and it is difficult to control; at the same time, the discretely distributed reinforcement phase is dispersed on the polylactic acid matrix, and the stability and continuity of the conductivity cannot be guaranteed. Summary of the invention

[0003] Purpose of the invention: The present invention aims to provide a polylactic acid composite material with excellent electrical conductivity, and the present invention also provides a method for preparing the conductive polylactic acid composite material.

[0004] Technical solution: The conductive polylactic acid composite material of the present invention comprises polylactic acid and graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface.

[0005] Furthermore, the mass ratio of the polylactic acid to the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface is 10:1-20:1, the silane coupling agent is one or more of KH560 and KH570, and the halogenated alkane side chains are one or more of R-CH2-Br and R-CH2-Cl.

[0006] The method for preparing the conductive polylactic acid composite material of the present invention comprises the following steps:

[0007] (1) adding graphene oxide with halogenated alkane side chains modified by a silane coupling agent into water and ultrasonically dispersing the graphene oxide solution to form a graphene oxide solution, and after the graphene oxide solution is uniformly dispersed, adding a copper nitrate solution and a silver nitrate solution, heating and dispersing the solution to obtain a mixed solution;

[0008] (2) adding nano Zn powder to the mixed solution, stirring the reaction, filtering and drying after the reaction is completed, thereby obtaining graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface;

[0009] (3) adding the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface obtained in step (2) to liquid polylactic acid, stirring and mixing, and then extruding and cooling to solidify, thereby obtaining a polylactic acid composite material rod-shaped wire;

[0010] (4) Loading the rod-shaped wire of the polylactic acid composite material into a fused deposition modeling machine, importing the three-dimensional data model of the conductive component, setting the molding process parameters, and performing fused deposition molding on the conductive component to obtain the conductive component.

[0011] Furthermore, in step (1), the concentration of the graphene oxide solution is 0.1-0.8 mol / L, the concentration of the copper nitrate solution is 0.02-0.08 mol / L, the concentration of the silver nitrate solution is 0.01-0.04 mol / L, and the volume ratio of the graphene oxide solution, the copper nitrate solution and the silver nitrate solution is 3:1:1 to 8:1:1; the temperature of heating and dispersion is 80-100°C.

[0012] Furthermore, in step (2), the mass of the nano Zn powder is 10-40 g, the particle size of the nano Zn powder is 10-100 nm, and the stirring reaction conditions are: temperature of 50-70° C., time of 20-60 min; and drying temperature of 80-110° C.

[0013] Furthermore, in step (3), the temperature of the liquid polylactic acid is 170-180°C.

[0014] Furthermore, in step (4), the process parameters of the fused deposition modeling are: the heating temperature is 120-180°C.

[0015] Principle of the invention: The present invention is aimed at the functional requirements of conductive polylactic acid formed by fused deposition molding. Based on the principle of material design, graphene oxide with halogenated alkane side chains modified by silane coupling agent is added to distilled water for ultrasonic dispersion, and then copper nitrate solution and silver nitrate solution are added to form a composite material solution; then nano Zn powder is added to the mixed solution and heated and ultrasonically stirred to induce GO / Zn, Zn / Cu 2+ 、Zn / Ag + In-situ reduction reaction GO+Zn→G+ZnO, Zn+Cu 2+ →Cu+Zn 2+ 、Zn+Ag + →Ag+Zn 2+, forming graphene oxide with surface loaded with nano zinc oxide and copper / silver particles; on this basis, adding it into liquid biodegradable polylactic acid and stirring it evenly with magnetic force, using the halogenated alkane side chains of graphene oxide modified with silane coupling agent to form a strong chemical bond with the carbonyl addition reaction of polylactic acid, thereby enhancing the bonding strength between functional graphene oxide and polylactic acid. At the same time, the highly conductive Cu, Ag and nano ZnO loaded on the surface of functional graphene oxide can significantly improve the conductive function of polylactic acid, thereby obtaining a special conductive material for fused deposition molding, solving the problem that there is currently no special conductive polylactic acid functional material, and providing a raw material basis for the fused deposition molding process of subsequent components; secondly, optimizing the molding process parameters according to the spatial structural characteristics of the conductive functional components, and performing precision molding of the complex structure conductive functional components through the fused deposition molding process based on the layer-by-layer accumulation principle, thereby realizing the precision manufacturing of complex structure conductive functional devices.

[0016] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0017] (1) Based on the spatial molecular structure of polylactic acid, the present invention uses graphene oxide modified with a silane coupling agent and having a halogenated alkane side chain, which can react with the carbonyl group of polylactic acid to form a strong chemical bond, thereby enhancing the bonding strength between the functional graphene oxide and polylactic acid, and providing a basis for obtaining good electrical conductivity;

[0018] (2) The present invention makes full use of graphene oxide / Zn, Zn / Cu 2+ 、Zn / Ag + Under the thermodynamic conditions of in-situ reduction, nano Zn particles are used to carry out in-situ reduction reaction on graphene oxide, copper ions and silver ions to form graphene oxide with surface loaded nano zinc oxide and copper / silver particles, wherein Cu, Ag, ZnO and graphene oxide all have good electrical conductivity, which can significantly improve the electrical conductivity of polylactic acid;

[0019] (3) The present invention adds graphene oxide with surface loaded nano zinc oxide, copper particles and silver particles into liquid polylactic acid and stirs it evenly to make it evenly dispersed in the liquid polylactic acid material matrix, and then extrudes the liquid polylactic acid composite material to solidify it into a rod-shaped wire material, thereby obtaining a conductive raw material specially used for fused deposition molding. This not only broadens the types and functions of raw materials specially used for fused deposition molding technology, but also further enriches the preparation process method of raw materials specially used for fused deposition molding technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a physical picture of the conductive polylactic acid composite rod-shaped wire material obtained in step (3) of Example 1 of the present invention;

[0021] Figure 2 The conductivity diagram of the conductive polylactic acid composite materials prepared in Examples 1 to 4 of the present invention and Comparative Examples 1 and 2. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below in conjunction with embodiments and drawings.

[0023] Example 1: The conductive polylactic acid composite material raw material of the present invention includes polylactic acid and modified graphene oxide with surface loaded nano zinc oxide, copper particles and silver particles, wherein the modified graphene oxide is graphene oxide with halogenated alkane side chains R-CH2-Br modified by KH560 silane coupling agent.

[0024] The preparation method of the conductive polylactic acid composite material is as follows:

[0025] (1) adding graphene oxide modified with a silane coupling agent and having a halogenated alkane side chain to distilled water for ultrasonic dispersion to form a graphene oxide solution with a concentration of 0.1 mol / L, adding a copper nitrate solution with a concentration of 0.02 mol / L and a silver nitrate solution with a concentration of 0.01 mol / L, wherein the volume ratio of the graphene oxide solution, the copper nitrate solution and the silver nitrate solution is 3:1:1, and heating to 80-100° C. to obtain a mixed solution;

[0026] (2) 10 g of 10 nm nano Zn powder was added to the mixed solution and magnetically stirred at 50 °C for 20 min to promote the GO / Zn and Zn / Cu 2+ 、Zn / Ag + The reaction was carried out in situ, and the reaction solution was filtered and dried at 80° C. to form graphene oxide modified with a silane coupling agent and having halogenated alkane side chains and loaded with nano zinc oxide, copper particles and silver particles on the surface;

[0027] (3) The graphene oxide with halogenated alkane side chains modified by silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface was added to the liquid polylactic acid at 170°C at a mass ratio of 10:1, and after being magnetically stirred evenly, it was extruded and water-cooled to solidify to obtain a conductive particle-reinforced polylactic acid composite rod-shaped wire, as shown in the actual figure. Figure 1 As shown;

[0028] (4) The conductive composite rod-shaped wire obtained in the above steps is loaded into a fused deposition modeling machine, a three-dimensional data model of the conductive component is imported, the molding process heating temperature is set to 120° C., and the conductive component is subjected to fused deposition molding to obtain a conductive polylactic acid composite material.

[0029] Example 2: The difference from Example 1 is that: in step (1), the concentration of the graphene oxide solution with halogenated alkane side chains modified by a silane coupling agent is set to 0.4 mol / L, and the volume ratio of the graphene oxide solution, the copper nitrate solution and the silver nitrate solution is 5:1:1; in step (4), the process heating temperature of the fused deposition molding is set to 180°C.

[0030] Example 3: The difference from Example 1 is that: in step (1), the concentrations of copper nitrate solution and silver nitrate solution are 0.05 mol / L and 0.02 mol / L respectively; in step (2), the mass of nano Zn powder is set to 20 g, the particle size is 100 nm, and the drying temperature is set to 100°C; in step (3), the mass ratio of polylactic acid and graphene oxide with halogenated alkane side chains modified by silane coupling agent and surface-loaded with nano zinc oxide, copper particles and silver particles is 20:1.

[0031] Example 4: The difference from Example 1 is that: in step (1), the concentration of the graphene oxide solution modified with a silane coupling agent and having halogenated alkane side chains is set to 0.8 mol / L, the concentrations of the copper nitrate solution and the silver nitrate solution are 0.08 mol / L and 0.04 mol / L, respectively, and the volume ratio of the graphene oxide solution, the copper nitrate solution and the silver nitrate solution is 8:1:1; in step (2), the mass of the nano Zn powder is set to 40 g.

[0032] Comparative Example 1: The difference from Example 1 is that the graphene oxide modified with a silane coupling agent and having halogenated alkane side chains is replaced with graphene oxide.

[0033] Comparative Example 2: The raw materials of the polylactic acid composite material are: 100g polylactic acid, 10g graphene oxide modified with a silane coupling agent and having halogenated alkane side chains, 20g ZnO, 16g Cu and 32g Ag.

[0034] The preparation method of the above-mentioned polylactic acid composite material is:

[0035] (1) adding 10 g of graphene oxide modified with a silane coupling agent and having a halogenated alkane branch, 20 g of ZnO, 16 g of Cu, and 32 g of Ag into liquid polylactic acid at 170° C., stirring the mixture uniformly with a magnetic force, and then extruding and water-cooling solidification to obtain a conductive particle-reinforced polylactic acid composite rod-shaped wire;

[0036] (2) The conductive composite rod-shaped wire obtained in the above steps is loaded into a fused deposition modeling machine, a three-dimensional data model of the conductive component is imported, the molding process heating temperature is set to 120° C., and the conductive component is subjected to fused deposition molding to obtain a polylactic acid composite material.

[0037] Figure 2The conductivity comparison diagram of the conductive polylactic acid composite material obtained in Example 1 to Example 4 shows that the conductivity is higher than 0.5S / m, which is much higher than the conductivity of the existing multi-walled carbon nanotube-enhanced polylactic acid composite material (0.012S / m). The conductivity of the polylactic acid composite material obtained in Comparative Example 1 and Comparative Example 2 is lower than the conductivity value in the embodiment. It further illustrates that the carbonyl addition reaction between the graphene oxide with halogenated alkane side chains modified by silane coupling agent and polylactic acid with high conductivity surface loading in the present method can significantly improve the conductive function of the functional component.

Claims

1. A conductive polylactic acid composite material, characterized in that: The raw materials include polylactic acid and graphene oxide with halogenated alkane branches and surface-loaded with nano zinc oxide, copper particles and silver particles and modified by a silane coupling agent; the preparation method of the conductive polylactic acid composite material includes the following steps: (1) adding graphene oxide with halogenated alkane side chains modified by a silane coupling agent to water for ultrasonic dispersion to form a graphene oxide solution, and after being evenly dispersed, adding copper nitrate solution and silver nitrate solution, heating and dispersing to obtain a mixed solution; (2) adding nano Zn powder to the mixed solution, stirring the reaction, filtering and drying after the reaction is completed, thereby obtaining graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface; (3) adding the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface obtained in step (2) to liquid polylactic acid, stirring and mixing, and then extruding and cooling to solidify, thereby obtaining a polylactic acid composite material rod-shaped wire; (4) Loading the rod-shaped wire of the polylactic acid composite material into a fused deposition modeling machine, importing the three-dimensional data model of the conductive component, setting the molding process parameters, and performing fused deposition molding on the conductive component to obtain the result.

2. The conductive polylactic acid composite material according to claim 1, characterized in that: The mass ratio of the polylactic acid to the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface is 10:1-20:

1.

3. The conductive polylactic acid composite material according to claim 1, characterized in that: The silane coupling agent is one or more of KH560 and KH570.

4. A method for preparing the conductive polylactic acid composite material according to claim 1, characterized in that: The following steps are involved: (1) adding graphene oxide with halogenated alkane side chains modified by a silane coupling agent to water for ultrasonic dispersion to form a graphene oxide solution, and after being evenly dispersed, adding copper nitrate solution and silver nitrate solution, heating and dispersing to obtain a mixed solution; (2) adding nano Zn powder to the mixed solution, stirring the reaction, filtering and drying after the reaction is completed, thereby obtaining graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface; (3) adding the graphene oxide with halogenated alkane side chains modified by a silane coupling agent and loaded with nano zinc oxide, copper particles and silver particles on the surface obtained in step (2) to liquid polylactic acid, stirring and mixing, and then extruding and cooling to solidify, thereby obtaining a polylactic acid composite material rod-shaped wire; (4) Loading the rod-shaped wire of the polylactic acid composite material into a fused deposition modeling machine, importing the three-dimensional data model of the conductive component, setting the molding process parameters, and performing fused deposition molding on the conductive component to obtain the result.

5. The preparation method according to claim 4, characterized in that: In step (1), the concentration of the graphene oxide solution is 0.1-0.8 mol / L, the concentration of the copper nitrate solution is 0.02-0.08 mol / L, the concentration of the silver nitrate solution is 0.01-0.04 mol / L, and the volume ratio of the graphene oxide solution, the copper nitrate solution and the silver nitrate solution is 3:1:1-8:1:

1.

6. The preparation method according to claim 4, characterized in that: In step (2), the mass of the nano Zn powder is 10-40 g, and the particle size of the nano Zn powder is 10-100 nm.

7. The preparation method according to claim 4, characterized in that: In step (2), the stirring reaction conditions are: temperature of 50-70° C. and time of 20-60 min.

8. The preparation method according to claim 4, characterized in that: In step (3), the temperature of the liquid polylactic acid is 170-180°C.

9. The preparation method according to claim 4, characterized in that: In step (4), the process parameters of the fused deposition modeling are: the heating temperature is 120-180°C.