Circularly polarized phosphorescent material, preparation method, application, and light-emitting device

Through ultrasonic treatment and magnetic field self-assembly technology, the chirality and structure of circularly polarized phosphorescent materials are controlled, solving the problems of uncontrollable chirality and material instability in the existing technology, achieving high luminescence asymmetry factor and stability, and is suitable for Optical anti-counterfeiting field.

CN116083073BActive Publication Date: 2024-10-11JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111308848.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-05
Publication Date
2024-10-11
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

The circularly polarized phosphorescent chirality of existing circularly polarized phosphorescent materials is uncontrollable, the luminescence asymmetry factor is low, and the material properties are unstable, which affects its application value in the field of optical anti-counterfeiting.

Method used

By regulating the energy density of the crystalline nanocellulose suspension by ultrasonic treatment, a circularly polarized phosphorescent material with controllable chirality is formed, and self-assembled under magnetic field conditions to obtain a silica-based composite film. The crystalline nanocellulose is removed after high-temperature calcination. Cellulose chiral template was used to obtain a silica-based circularly polarized phosphorescent material with an inverse topological chiral nematic phase structure.

Benefits of technology

It achieves controllable chirality and stability of material properties of circularly polarized phosphorescent materials, improves the luminescence asymmetry factor, enhances circularly polarized signals, is suitable for different levels of optical anti-counterfeiting applications, and increases recognition and application stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116083073B_ABST
    Figure CN116083073B_ABST
Patent Text Reader

Abstract

The invention discloses a circularly polarized phosphorescent material, a preparation method, an application, and a light-emitting device. The preparation method of the circularly polarized phosphorescent material comprises: placing a mixed solution of a crystalline nanocellulose suspension treated with ultrasound and an organic silane precursor in a horizontal magnetic field, self-assembling at room temperature, and obtaining a crystalline nanocellulose@silicon dioxide composite film after the water in the mixed solution is completely evaporated; calcining the crystalline nanocellulose@silicon dioxide composite film to obtain a silicon dioxide-based circularly polarized phosphorescent material; the energy density range of the ultrasound treatment is 65 J·g ‑1 ~2300 J·g ‑1 The preparation method is simple, and the prepared circularly polarized phosphorescent material has stable properties, a more regular chiral nematic phase structure and a higher asymmetry factor, as well as significant circularly polarized room temperature phosphorescence properties and excellent optical regulation capabilities, which can meet different levels of anti-counterfeiting needs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention specifically relates to a circularly polarized phosphorescent material, a preparation method, an application, and a light-emitting device. Background Art

[0002] In recent years, circularly polarized room temperature phosphorescent materials have gradually come into people's view. Their long afterglow and special chiral optical properties make them have excellent potential application value in optical information encryption, biological imaging and optoelectronic devices.

[0003] At present, most circularly polarized room temperature phosphorescent materials are derived from chiral organic metal complexes, such as platinum metal complexes of helicene ligands, rhenium metal complexes, chiral iridium metal ligand complexes, cyclometallated platinum complexes disclosed in CN111187300A, and organic compounds used in

[0012] and

[0013] of CN113121410A, etc. In addition, pure organic luminescent materials designed and synthesized by chiral ester-linked carbazole also have certain circularly polarized room temperature phosphorescent properties. Unfortunately, the preparation of these materials usually requires complex molecular design and lengthy synthesis processes, the chirality of their circularly polarized phosphorescence is unpredictable, and they have a low luminescence asymmetry factor (g lum , luminescence dissymmetry factor), etc., which to some extent affect the practical application value of circularly polarized phosphorescent materials.

[0004] Cellulose is a natural high molecular polymer. Crystalline nanocellulose obtained by sulfuric acid hydrolysis can form a self-supporting film material with a chiral nematic phase structure through evaporation-induced self-assembly. Its special periodic spiral arrangement enables it to selectively reflect left-handed circularly polarized light in a specific band. Liu et al. used this property to composite crystalline nanocellulose with carbon dots with room temperature phosphorescent properties to prepare a film material with circularly polarized phosphorescent properties. This method is simple and convenient, and has good biocompatibility, but the cellulose-based film material itself will disassemble when it comes into contact with water, and the destruction of the structure becomes a disadvantage.

[0005] CN109438770A discloses a circularly polarized up-conversion luminescent film based on chiral nematic cellulose nanocrystals and a preparation method thereof, and CN107987291B discloses a circularly polarized luminescent material based on crystalline nanocellulose, a preparation method and its application in anti-counterfeiting. The circularly polarized luminescent materials in these two prior arts both contain crystalline nanocellulose and have the above-mentioned disadvantages.

[0006] In 2010, MacLachlan et al. successfully introduced chiral nematic phase structure into inorganic materials by co-assembling crystalline nanocellulose and silicon source precursors, using crystalline nanocellulose as a chiral template, and obtained a self-supporting silica film material with periodic spiral arrangement of anti-topological crystalline nanocellulose. And by adjusting the ratio of silicon source to crystalline nanocellulose, the reflection of circularly polarized light of different wavelengths can be adjusted.

[0007] Silica-based materials are a large class of defect-induced photoluminescent materials with a variety of defect-state luminescence properties. The phosphorescence phenomenon caused by ODC-type oxygen defect centers has not yet been applied in circularly polarized optical materials.

[0008] Based on the above, it can be seen that the circularly polarized phosphorescent materials involved in the prior art have problems such as uncontrollable chirality of circularly polarized phosphorescent light, low luminescence asymmetry factor, and unstable phosphorescent properties. As far as we know, there is currently no technology involving direct regulation of the chirality of circularly polarized phosphorescent materials, and chiral materials based on silicon sources have not yet been involved in this aspect, which plays an important role in the field of anti-counterfeiting. Therefore, there is an urgent need for a circularly polarized phosphorescent material based on silicon dioxide that has controllable chiral circularly polarized phosphorescent light and a high luminescence asymmetry factor. Summary of the invention

[0009] The technical problem to be solved by the present invention is that in the field of circularly polarized phosphorescent materials, the circularly polarized phosphorescent materials have defects such as uncontrollable chirality of circularly polarized phosphorescent light, unstable material properties, and low luminescence asymmetry factor. A circularly polarized phosphorescent material, a preparation method, an application, and a light-emitting device are provided. The circularly polarized phosphorescent material has circularly polarized phosphorescence with controllable chirality, and at the same time has a high luminescence asymmetry factor, stable material properties, and can be suitable for different levels of optical anti-counterfeiting.

[0010] The inventors of the present invention have discovered that the circularly polarized phosphorescent material of the present invention produces defective phosphorescence due to high-temperature calcination. Further research has found that by changing the energy density of the ultrasonic treatment of the crystalline nanocellulose suspension, the photon bandgap position of the chiral nematic phase structure of the circularly polarized phosphorescent material can be adjusted, thereby adjusting the chirality of the circularly polarized room temperature phosphorescence; when the defective phosphorescence emission peak coincides with the photon bandgap peak, right-handed circularly polarized phosphorescence is obtained; when the defective phosphorescence emission peak is located at the photon bandgap band edge, left-handed circularly polarized phosphorescence is obtained. ; When the defect state phosphorescence emission peak and the photon bandgap peak are between the above two situations, right-handed and left-handed circularly polarized phosphorescence are obtained at the same time, and it is also accidentally discovered that the crystalline nanocellulose@silica composite film induced by self-assembly under magnetic field conditions, and then calcined to remove the crystalline nanocellulose chiral template, the obtained silica-based circularly polarized phosphorescent material with an anti-topological chiral nematic phase structure has a more regular chiral nematic phase structure, a higher asymmetry factor, and a stronger circular polarization signal. When used in the anti-counterfeiting field, it can achieve a higher recognition degree.

[0011] The present invention solves the above technical problems through the following technical solutions:

[0012] The present invention provides a method for preparing a circularly polarized phosphorescent material, which comprises the following steps:

[0013] Placing a mixed solution of an ultrasonically treated crystalline nanocellulose suspension and an organosilane precursor in a horizontal magnetic field for self-assembly at room temperature, and obtaining a crystalline nanocellulose@silicon dioxide composite film after the water in the mixed solution is completely evaporated;

[0014] The crystalline nanocellulose@silicon dioxide composite film is calcined to obtain a silicon dioxide-based circularly polarized phosphorescent material;

[0015] The energy density range of the ultrasonic treatment is 65 J·g -1 ~2300 J·g -1 .

[0016] In the present invention, the “complete evaporation of water” refers to the complete evaporation of water observable by the naked eye of a person skilled in the art.

[0017] In the present invention, the crystalline nanocellulose suspension can be obtained by conventional methods in the art, for example, by hydrolysis of cellulose. The cellulose may include one of wood cellulose, non-wood cellulose and bacterial cellulose. The non-wood cellulose preferably includes cotton pulp cellulose and / or herbaceous cellulose, and the non-wood cellulose is preferably cotton pulp cellulose. These types of cellulose are all commercially available. The hydrolysis method may be acid hydrolysis. The acid used in the acid hydrolysis preferably includes sulfuric acid.

[0018] In the present invention, the energy density of the ultrasonic treatment is generally equal to the product of the power of the ultrasonic treatment and the time of the ultrasonic treatment divided by the mass of the crystalline nanocellulose.

[0019] In the present invention, the mass fraction of the crystalline nanocellulose suspension is generally 2% to 6%.

[0020] In the present invention, the pH value of the crystalline nanocellulose suspension is preferably 1 to 3, for example, the pH value is 2. The pH value can be adjusted by adding acid. The acid can include one or more of formic acid, acetic acid, citric acid and hydrochloric acid.

[0021] In the present invention, the ultrasonic treatment method can be conventional in the art, such as an ultrasonic cell disruptor. The power of the ultrasonic cell disruptor is generally 15W to 20W.

[0022] In the present invention, the ultrasonic treatment time is preferably 1s to 35s, more preferably 1s to 25s, and further more preferably 2s to 21s.

[0023] In the present invention, the energy density range of the ultrasonic treatment is preferably 266.7 J·g -1 or 533.3 J·g -1 .

[0024] In the present invention, the mass ratio of the crystalline nanocellulose suspension to the organosilane precursor is preferably 1:(1-3).

[0025] In the present invention, the organosilane precursor preferably includes tetramethoxysilane or tetraethoxysilane.

[0026] In the present invention, the "mixed solution of ultrasonically treated crystalline nanocellulose suspension and organosilane precursor" can generally be obtained by stirring, preferably by stirring until no obvious oil droplets are present. The stirring time is generally 1 hour to 3 hours.

[0027] In the present invention, the "mixed solution of ultrasonically treated crystalline nanocellulose suspension and organosilane precursor" is generally contained in a culture dish. The specification of the culture dish can be 3 cm to 4 cm in diameter, for example, 3.5 cm. The material of the culture dish can be polystyrene.

[0028] In the present invention, the calcination method can be conventional in the art, such as muffle furnace calcination. The calcination temperature is preferably 500° C. to 600° C., such as 550° C. The calcination time is preferably 5 h to 7 h, more preferably 6 h.

[0029] In the present invention, the magnetic field strength of the horizontal magnetic field is preferably in the range of 0.5T to 5T, more preferably in the range of 0.6T to 2T, and even more preferably in the range of 0.6T to 1T.

[0030] In the present invention, the room temperature generally refers to 10°C to 30°C.

[0031] The present invention also provides a circularly polarized phosphorescent material, which is prepared by the above preparation method.

[0032] In the present invention, the photon bandgap peak wavelength range of the circularly polarized phosphorescent material is preferably 445nm to 900nm.

[0033] In the present invention, the absolute value of the luminescence asymmetry factor of the circularly polarized phosphorescent material is preferably 0.10 to 0.2, such as 0.13.

[0034] The present invention also provides a light-emitting device, which comprises the circularly polarized phosphorescent material.

[0035] The present invention also provides an application of the circularly polarized phosphorescent material in optical anti-counterfeiting.

[0036] In the present invention, preferably, the circularly polarized phosphorescent material is used as an optical label in optical anti-counterfeiting.

[0037] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0038] The reagents and raw materials used in the present invention are commercially available.

[0039] The positive and progressive effects of the present invention are:

[0040] (1) Wide sources of raw materials: Crystalline nanocellulose can be obtained through conventional cellulose hydrolysis.

[0041] (2) The preparation method is simple: the preparation process does not require the introduction of a large amount of chemical substances or the additional synthesis of organic molecules.

[0042] (3) Stable material properties: The circularly polarized phosphorescent material of the present invention is insoluble in water, resistant to high temperatures, and resistant to acid and alkali corrosion (stable in most polar and non-polar solvents except concentrated solutions of strong acids and alkalis and hydrofluoric acid), and has stable phosphorescent properties. Triplet excitons will not be quenched by oxygen (no need to introduce triplet stabilizers, etc.).

[0043] (4) Significant circularly polarized room temperature phosphorescence properties and excellent optical control capabilities: The optical label made of the circularly polarized phosphorescent material of the present invention has a superposition of multiple circularly polarized optical signals, and the color of the circularly polarized phosphorescent material can span the visible to near-infrared band; the optical label can not only be identified by the human eye, but also can be accurately identified by instrument detection, with a higher degree of recognition, meeting the requirements of different anti-counterfeiting levels. Such rich optical properties increase the difficulty of imitation.

[0044] (5) The chiral nematic phase structure of the circularly polarized phosphorescent material of the present invention is more regular and has a higher asymmetry factor. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The transmission spectra of the circularly polarized phosphorescent material prepared in Comparative Example 1 under different ultrasonic conditions (according to the peak position, from left to right are Comparative Example 1-1 to Comparative Example 1-9)).

[0046] Figure 2 The scanning electron microscope image of the cross section of the crystalline nanocellulose@silicon dioxide composite membrane of Examples 1-10 ( Figure 2 (A)); and scanning electron microscopy images of the cross-section of the circularly polarized phosphorescent material ( Figure 2 (B)).

[0047] Figure 3 Schematic diagram of the internal structure of the circularly polarized phosphorescent material of the present invention and the relationship between the controllable chirality of circularly polarized room temperature phosphorescence and the position of the photon band gap ("R-CTRTP": right-handed circularly polarized room temperature phosphorescence, "L-CPRTP": left-handed circularly polarized room temperature phosphorescence).

[0048] Figure 4 Circular dichroism spectra of the circularly polarized phosphorescent materials of Comparative Examples 1-2, 1-6 and 1-9.

[0049] Figure 5 It is the phosphorescence spectrum diagram of the circularly polarized phosphorescent materials of comparative examples 1-1 to 1-9.

[0050] Figure 6 Circularly polarized phosphorescence spectra of the circularly polarized phosphorescent materials of Comparative Examples 1-1 to 1-9.

[0051] Figure 7 The circularly polarized phosphorescent material transmission spectra and phosphorescence spectra of Examples 1-10 and 1-11 are shown in FIG. Figure 7(A)), Circularly polarized phosphorescence spectrum ( Figure 7 (B)).

[0052] Figure 8 This is an optical encryption label for application demonstration of the circularly polarized phosphorescent material in Comparative Example 1. In the figure, "L-CPF" represents a left-handed circular polarizer (400nm-700nm band), and "R-CPF" represents a right-handed circular polarizer (400nm-700nm band). DETAILED DESCRIPTION

[0053] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0054] The power used by the ultrasonic cell disruptor in the following examples and comparative examples is 20W.

[0055] Example 1

[0056] Preparation of circularly polarized room temperature phosphorescent films based on silica under magnetic field conditions:

[0057] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for a certain time, add acetic acid to adjust the suspension pH to 2, then add 400μL tetramethoxysilane (mass ratio 1:1), and continue stirring for 1 hour until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, place it in parallel in an external horizontal magnetic field, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film was calcined at 550℃ in air for 6 hours to obtain a circularly polarized room temperature phosphorescent film based on silica under magnetic field conditions.

[0058] The above-mentioned ultrasound constant time is 4s and 8s, respectively, corresponding to Example 1-10 and Example 1-11, and the applied horizontal magnetic field strength is 0.6T.

[0059] Comparative Example 1

[0060] Preparation of circularly polarized room temperature phosphorescent films based on silicon dioxide with different photon band gaps:

[0061] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for a certain time, add formic acid to adjust the suspension pH to 2, then add 400μL tetramethoxysilane (mass ratio 1:1), and continue stirring for 1 hour until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0062] The above-mentioned ultrasound certain time is 3s, 4s, 5s, 7s, 9s, 11s, 13s, 15s, 21s, corresponding to proportions 1-1, 1-2, 1-3, 1-4, 1-5, 1-6, 1-7, 1-8, 1-9, respectively.

[0063] Comparative Example 2: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0064] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add acetic acid to adjust the suspension pH to 2, then add 400μL tetramethoxysilane (mass ratio 1:1), and continue stirring for 1 hour until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0065] Comparative Example 3: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0066] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add hydrochloric acid to adjust the suspension pH to 2, then add 400μL tetramethoxysilane (mass ratio 1:1), and continue stirring for 1 hour until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0067] Comparative Example 4: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0068] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add citric acid to adjust the suspension pH to 2, then add 400μL tetramethoxysilane (mass ratio 1:1), and continue stirring for 1 hour until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0069] Comparative Example 5: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0070] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add formic acid to adjust the suspension pH to 2, then add 600μL tetraethoxysilane (mass ratio 1:1), and continue stirring for 3 hours until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0071] Comparative Example 6: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0072] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add acetic acid to adjust the suspension pH to 2, then add 600μL tetraethoxysilane (mass ratio 1:1), and continue stirring for 3 hours until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0073] Comparative Example 7: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0074] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add hydrochloric acid to adjust the suspension pH to 2, then add 600μL tetraethoxysilane (mass ratio 1:1), and continue stirring for 3 hours until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0075] Comparative Example 8: Preparation of Circularly Polarized Room Temperature Phosphorescent Film Based on Silica:

[0076] Take 10g of 3% sulfuric acid hydrolyzed crystalline nanocellulose suspension, use ultrasonic cell disruptor for 4s, add citric acid to adjust the suspension pH to 2, then add 600μL tetraethoxysilane (mass ratio 1:1), and continue stirring for 3 hours until no obvious oil droplets appear. Pour the mixed stable solution into a 3.5cm diameter polystyrene petri dish, self-assemble at room temperature, and form a crystalline nanocellulose@silica composite film after water evaporation. The composite film is calcined at 550℃ in air for 6 hours to obtain a silica-based circularly polarized room temperature phosphorescent film.

[0077] Effect Example 1

[0078] The circularly polarized phosphorescent materials in Comparative Example 1 (Comparative Examples 1-1 to 1-9) were tested by UV-visible spectrometer to obtain Figure 1 ,from Figure 1 It can be seen that the photon bandgap of circularly polarized phosphorescent materials is adjustable in the visible to near-infrared range, with a peak position of 455nm to 900nm.

[0079] The circularly polarized phosphorescent materials in Examples 1-10 were tested by field emission scanning electron microscopy to obtain Figure 2 Scanning electron microscope image of Figure 2 (A) It can be seen that the crystalline nanocellulose@silica composite film before calcination has formed a chiral nematic structure, while the circularly polarized phosphorescent material obtained after calcination ( Figure 2 (B)) still retains the chiral nematic structure, and the chiral nematic structure is regular.

[0080] Figure 3 Schematic diagram of the internal structure of the circularly polarized phosphorescent material of the present invention and the relationship between the controllable chirality of circularly polarized room temperature phosphorescence and the position of the photon band gap ("R-CTRTP": right-handed circularly polarized room temperature phosphorescence, "L-CPRTP": left-handed circularly polarized room temperature phosphorescence).

[0081] The circularly polarized phosphorescent materials in Comparative Examples 1-2, 1-6 and 1-9 were tested by an Applied Photophysics Chirascan V100 circular dichroism spectrometer to obtain Figure 4 The circular dichroism spectrum is characterized by the phosphorescence emission wavelength position coinciding with the photon bandgap, being located at the edge of the photon bandgap and being far away from the photon bandgap; the positive peak signal in the circular dichroism spectrum indicates that the circularly polarized phosphorescent material has a left-handed chiral structure.

[0082] The circularly polarized phosphorescent materials of Comparative Examples 1-1 to 1-9 were tested by FLS920 fluorescence spectrometer and obtained Figure 5 The phosphorescence spectrum and phosphorescence lifetime table are shown in Table 1.

[0083] Table 1

[0084]

[0085] In the table, "CNS-PBG" represents a circularly polarized room temperature phosphorescent material of silicon dioxide with a chiral nematic phase structure and a photon bandgap position of PBG nm, for example, "CNS-445" represents a circularly polarized room temperature phosphorescent material of silicon dioxide with a chiral nematic phase structure and a photon bandgap position of 455 nm.

[0086] The circularly polarized phosphorescent materials of Comparative Examples 1-1 to 1-9 were tested by a JASCO CPL-200 spectrophotometer to obtain Figure 6 The circularly polarized phosphorescence spectrum and Table 2. As shown in Table 2, there is no circularly polarized phosphorescence signal in Comparative Examples 1-7 to 1-9, and the calculation formula is: g lum =2(I L -I R ) / (I L +I R ), where I L ,I R are the left- and right-handed circularly polarized phosphorescence intensities, respectively.

[0087] Table 2

[0088]

[0089]

[0090] In the table, “--” indicates that there is no circularly polarized phosphorescence signal.

[0091] The circularly polarized phosphorescent materials of Examples 1-10 and 1-11 were tested in the same manner as above and obtained Figure 7 (A) The transmission spectrum and phosphorescence spectrum (the dashed line curve represents the phosphorescence spectrum with a peak at 440 nm), and Figure 7(B) is a circularly polarized phosphorescence spectrum diagram; in the diagram, the phosphorescence peak of the circularly polarized phosphorescent material of Examples 1-10 coincides with the photon bandgap (peak 445nm), and the phosphorescence peak of the circularly polarized phosphorescent material of Examples 1-10 is located at the band edge of the photon bandgap (peak 541nm). Figure 7 It can be seen from the transmission spectrum of (A) that compared with the transmission spectrum of Comparative Example 1, the half-peak widths in Examples 1-10 and 1-11 are narrower, proving that the structures are more regular. Figure 7 From the phosphorescence spectrum of (A), it can be seen that the half-peak width of the photon bandgap of the circularly polarized phosphorescent material becomes narrower under magnetic field conditions. Figure 7 (B) Circularly polarized phosphorescence spectrum, showing the asymmetry factor g of circularly polarized phosphorescence under magnetic field conditions. lum The absolute value has increased to 0.13.

[0092] Effect Example 2

[0093] The circularly polarized phosphorescent materials of Comparative Examples 1-1 to 1-9 were encapsulated in two 25 mm × 25 mm × 0.5 mm quartz sheets to form a 3 × 3 color card for optically encrypted label display, such as Figure 8 As shown (in the figure: "L-CPF" represents left-handed circular polarizer, and "R-CPF" represents right-handed circular polarizer). Figure 8 (A) Schematic diagram of a 3×3 color card, 1 to 9 are respectively the non-circularly polarized phosphorescent materials in comparative examples 1-1 to 1-9, and the dotted line is the boundary of the encapsulated quartz plate; Figure 8 (B) Under the white background, the color card is almost completely transparent, and the writing on the white paper below can be clearly seen; Figure 8 (C) Under a black background, due to the absorption of the transmitted light by the black background, the selective reflection colors of circularly polarized phosphorescent materials with different photon band gaps (spanning the visible region to the near-infrared band) are observed (1-blue, 2-blue-green, 3-yellow-green, 4-orange-yellow, 5-orange, 6-orange-red, 7-red, 8-dark red, 9-colorless). Figure 8 (E) Place a left-handed circular polarizer on top of the color card. These selective emission colors are more vivid and have higher contrast. Figure 8 (F) When a right-handed circular polarizer is placed on top of the color card, the color card appears colorless and no selective reflection color can be observed; Figure 8 (D) Under ultraviolet light (254nm), the color card appears bright blue as a whole, but the luminous intensity of each module is different. Figure 8 (G) After removing the excitation light source, a phosphorescence afterglow lasting several seconds can be observed.

Claims

1. A method for preparing a circularly polarized phosphorescent material, characterized in that: It includes the following steps: Placing a mixed solution of an ultrasonically treated crystalline nanocellulose suspension and an organosilane precursor in a horizontal magnetic field, self-assembling at room temperature, and obtaining a crystalline nanocellulose@silicon dioxide composite film after the water in the mixed solution is completely evaporated; the magnetic field strength of the horizontal magnetic field ranges from 0.5T to 5T; and the organosilane precursor is tetramethoxysilane or tetraethoxysilane; The crystalline nanocellulose@silicon dioxide composite film is calcined to obtain a silicon dioxide-based circularly polarized phosphorescent material; The energy density range of the ultrasonic treatment is 65 J·g -1 ~2300 J·g -1 .

2. The method for preparing a circularly polarized phosphorescent material according to claim 1, characterized in that: The ultrasonic treatment time is 1s to 35s; And / or, the magnetic field strength of the horizontal magnetic field is 0.6T to 2T; and / or, the mass ratio of the crystalline nanocellulose suspension to the organosilane precursor is 1:(1-3); And / or, the energy density range of the ultrasonic treatment is 266.7 J·g -1 or 533.3 J·g -1 .

3. The method for preparing a circularly polarized phosphorescent material according to claim 2, characterized in that: The ultrasonic treatment time is 1s to 25s.

4. The method for preparing a circularly polarized phosphorescent material according to claim 3, characterized in that: The ultrasonic treatment time is 2s to 21s.

5. The method for preparing a circularly polarized phosphorescent material according to claim 2, characterized in that: The magnetic field strength of the horizontal magnetic field is 0.6T to 1T.

6. The method for preparing a circularly polarized phosphorescent material according to claim 1, characterized in that: The mass fraction of the crystalline nanocellulose suspension is 2% to 6%; and / or, the crystalline nanocellulose suspension is obtained by hydrolyzing cellulose; And / or, the pH value of the crystalline nanocellulose suspension is 1-3.

7. The method for preparing a circularly polarized phosphorescent material according to claim 6, characterized in that: The cellulose is one of woody cellulose, non-woody cellulose and bacterial cellulose.

8. The method for preparing a circularly polarized phosphorescent material according to claim 7, characterized in that: The non-woody cellulose is cotton pulp cellulose and / or herbaceous cellulose.

9. The method for preparing a circularly polarized phosphorescent material according to claim 8, characterized in that: The non-woody cellulose is cotton pulp cellulose.

10. The method for preparing a circularly polarized phosphorescent material according to claim 6, characterized in that: The hydrolysis method is acid hydrolysis.

11. The method for preparing a circularly polarized phosphorescent material according to claim 10, characterized in that: The acid used in the acid hydrolysis is sulfuric acid.

12. The method for preparing a circularly polarized phosphorescent material according to claim 6, characterized in that: The pH value of the crystalline nanocellulose suspension is 2.

13. The method for preparing a circularly polarized phosphorescent material according to claim 12, characterized in that: The pH value was adjusted by adding acid.

14. The method for preparing a circularly polarized phosphorescent material according to claim 13, characterized in that: The acid is one or more of formic acid, acetic acid, citric acid and hydrochloric acid.

15. The method for preparing a circularly polarized phosphorescent material according to claim 1, characterized in that: The ultrasonic treatment is carried out by using an ultrasonic cell disruptor.

16. The method for preparing a circularly polarized phosphorescent material according to claim 15, characterized in that: The power of the ultrasonic cell disruptor is 15W-20W.

17. The method for preparing a circularly polarized phosphorescent material according to claim 1, characterized in that: The "mixed solution of ultrasonically treated crystalline nanocellulose suspension and organosilane precursor" is obtained by stirring; And / or, the "mixed solution of ultrasonic crystalline nanocellulose suspension and organosilane precursor" is contained in a culture dish.

18. The method for preparing a circularly polarized phosphorescent material according to claim 17, characterized in that: The "mixed solution of ultrasonically treated crystalline nanocellulose suspension and organosilane precursor" is obtained by stirring until no obvious oil droplets are present.

19. The method for preparing a circularly polarized phosphorescent material according to claim 18, characterized in that: The stirring time is 1 h to 3 h.

20. The method for preparing a circularly polarized phosphorescent material according to claim 17, characterized in that: The specification of the culture dish is 3cm to 4cm in diameter.

21. The method for preparing a circularly polarized phosphorescent material according to claim 20, characterized in that: The specification of the culture dish is 3.5 cm in diameter.

22. The method for preparing a circularly polarized phosphorescent material according to claim 17, characterized in that: The material of the culture dish is polystyrene.

23. The method for preparing a circularly polarized phosphorescent material according to claim 1, characterized in that: The calcination method is muffle furnace calcination; And / or, the room temperature is 10°C to 30°C.

24. The method for preparing a circularly polarized phosphorescent material according to claim 23, characterized in that: The calcination temperature is 500°C to 600°C.

25. The method for preparing a circularly polarized phosphorescent material according to claim 24, characterized in that: The calcination temperature is 550°C.

26. The method for preparing a circularly polarized phosphorescent material according to claim 23, characterized in that: The calcination time is 5h to 7h.

27. The method for preparing a circularly polarized phosphorescent material according to claim 26, characterized in that: The calcination time is 6 hours.

28. A circularly polarized phosphorescent material, characterized in that: The circularly polarized phosphorescent material is prepared by the method for preparing the circularly polarized phosphorescent material as claimed in any one of claims 1 to 27.

29. The circularly polarized phosphorescent material according to claim 28, characterized in that The photon bandgap peak wavelength range of the circularly polarized phosphorescent material is 445nm to 900nm; And / or, the absolute value of the luminescence asymmetry factor of the circularly polarized phosphorescent material is 0.10-0.

20.

30. The circularly polarized phosphorescent material according to claim 29, characterized in that The absolute value of the luminescence asymmetry factor of the circularly polarized phosphorescent material is 0.

13.

31. A light emitting device, characterized in that: It comprises the circularly polarized phosphorescent material as claimed in claim 28.

32. Use of the circularly polarized phosphorescent material according to claim 28 in optical anti-counterfeiting.

33. Use of the circularly polarized phosphorescent material in optical anti-counterfeiting as claimed in claim 32, characterized in that: The circularly polarized phosphorescent material is used as an optical label in optical anti-counterfeiting.