A fiber dyeing method for improving color yield and color saturation

Through the reaction of epoxy quaternary ammonium salt and cellulose fibers, the low dyeing fixation rate and pollution problems in traditional reactive dye dye dyeing are solved, and efficient dye adsorption and dyeing effects are achieved, reducing pollution and cost.

CN116084188BActive Publication Date: 2024-11-26DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310061614.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-11-26
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

During the dyeing process of traditional reactive dyes, the dyeing and color fixation rate is low due to the repulsion of anionic groups and cellulose fibers, and the need for a large amount of inorganic salt additives leads to contamination and low dye utilization rate.

Method used

Epoxy quaternary ammonium salt is synthesized by reacting epoxy chloride with tertiary amine, reacting with cellulose fibers as cationic modifiers, controlling the reaction conditions to improve the quaternization rate and epoxy value, and using a dyeing additive combined with multiple additives Method: reduce the amount of modifier and increase the adsorption depth of dye.

Benefits of technology

It has achieved a high dye utilization rate of nearly 100%, no need to add inorganic salts, reducing the difficulty and cost of treating polluted wastewater, and the fibers are darker in color, higher saturation after dyeing, and good dyeing uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses a fiber dyeing method for improving color yield and color saturation, comprising the following steps: S1, adding soaked cellulose fiber to an aqueous solution of an epoxy quaternary ammonium salt composition and an alkali agent, with a bath ratio of 1:3-5, then sealing and reacting at 30-40°C, heating to 60-80°C to continue the reaction, washing with water, and obtaining modified fiber; S2, placing the modified fiber in a dye bath with a chromaticity of 1-6% (owf), with a bath ratio of 1:5-25, first dyeing at 30-40°C, then heating to 60-70°C, continuing dyeing, washing with water, soaping, with a bath ratio of 1:50, then washing with water, and drying. The method of the invention can simultaneously improve the dye penetration and apparent depth of the dye, not only realizing the improvement of the color yield without adding salt, but also reducing the amount of modifier, improving the color saturation, and better meeting the application requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile printing and dyeing, and in particular relates to a method for cationized modified dyeing of cellulose fibers with no salt, high color yield and high color saturation. Background Art

[0002] Reactive dyes are widely used in the dyeing process of cotton, viscose and their blended fibers due to their advantages of complete color spectrum, low cost, bright color and simple dyeing process. In the reactive dyeing process, the dye is mainly adsorbed to the fiber surface by the fiber's affinity for it, and then diffuses into the fiber to react and complete the dyeing. However, due to the presence of anionic groups in the molecular structure of reactive dyes, they are negatively charged in water and will repel cellulose fibers in water that are also negatively charged, resulting in a low fixation rate of reactive dyeing.

[0003] Traditional reactive dyeing is to add a large amount of inorganic salts (such as sodium sulfate) to the dye bath, and the salt dosage is generally 30-100g / L, which leads to a large amount of inorganic salts in the dyeing wastewater. If it is directly discharged, it will change the water quality of rivers and lakes, causing soil salinization and seriously affecting the growth of crops. In addition, the traditional method of adding inorganic salts ultimately achieves a dye utilization rate of only 50% to 70%, resulting in a large amount of dye waste and the discharge of colored wastewater.

[0004] In response to the problems of salt pollution and color pollution caused by reactive dyes, the salt-free dyeing methods at home and abroad mainly include using new solvent systems, developing cationic reactive dyes, and using salt-free dyeing auxiliaries to modify the structure of fibers. The existing solvent system mainly uses organic solvents as dyeing solvents, which have safety hazards and high costs during use; while the cationic reactive dyes developed by the existing technology have a narrow application range and will change the molecular structure of the dyes, causing changes in color. Summary of the invention

[0005] The present invention provides a method for reducing the amount of modifier and effectively improving the fiber dyeing depth and apparent color yield, so as to promote the adsorption of dyes, ensure the surface dyeing and through dyeing of dyes, and develop a dyeing auxiliary agent combined with multiple auxiliary agents.

[0006] The present invention synthesizes a series of epoxy quaternary ammonium salts by reacting epichlorohydrin with tertiary amine, and the quaternization rate and epoxy value are optimized by controlling the reaction conditions. The reaction route and principle of the present invention are as follows:

[0007]

[0008] The present invention provides a fiber dyeing method, comprising the following steps:

[0009] S1, adding the soaked cellulose fiber to an aqueous solution of an epoxy quaternary ammonium salt composition and an alkali agent at a bath ratio of 1:3-5, and then sealing and reacting at 30-40°C, then heating to 60-80°C to continue the reaction, and washing with water to obtain a modified fiber;

[0010] S2. Place the modified fiber in a dye bath with a chroma of 1-6% (owf) and a bath ratio of 1:5-25, first dye at 30-40°C, then heat to 60-70°C, continue dyeing, wash with water, soap, use a bath ratio of 1:50, wash again with water, and air dry.

[0011] Preferably, the preparation method of the epoxy quaternary ammonium salt comprises:

[0012] S1. Under nitrogen protection, epichlorohydrin is added dropwise to a tertiary amine dissolved in an organic solvent, mixed evenly at 0-25°C, and heated to 25-60°C to react until the product no longer increases; the tertiary amine is one of formulas Ⅰ, Ⅱ, Ⅲ, and Ⅳ:

[0013]

[0014] Wherein R1 is an alkyl group with a length of 10 to 18, R2 is an alkyl group with a length of 1 to 6, and n is an integer of 2 to 6;

[0015] S2. Purify and remove impurities, then elute with anhydrous petroleum ether, and then vacuum dry at 30-40°C to obtain the epoxy quaternary ammonium salt corresponding to the tertiary amine of type I, II, III or IV.

[0016] Preferably, in step S1, the reaction is carried out at 30-40°C for 20-30 minutes under a sealed state, and the temperature is raised to 60-80°C for further reaction for 10-30 minutes; in step S2, dyeing is carried out at 30-40°C for 20-30 minutes, and then the temperature is raised to 60-70°C, and dyeing is further carried out for 30-40 minutes; the water washing is performed 1-2 times; and the soap washing includes soap washing with a soap solution having a mass fraction of 2‰ using standard soap flakes.

[0017] Preferably, the organic solvent is one of methanol, ethanol or ethyl acetate; the mass ratio of the organic solvent to epichlorohydrin is 1:2-3.

[0018] Preferably, the purification and impurity removal method comprises distillation under reduced pressure at 60-75°C.

[0019] Preferably, the alkali agent in step S1 comprises one or more combinations of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate; the mass ratio of the alkali agent to the epoxy quaternary ammonium salt is 0.1 to 0.5:1.

[0020] Preferably, the epoxy quaternary ammonium salt composition in step S1 includes Class I epoxy quaternary ammonium salt and one of Class II, III or IV epoxy quaternary ammonium salts, wherein the mass ratio of Class I epoxy quaternary ammonium salt to cellulose fiber is 0.06-0.1:1; the mass ratio of Class II, III or IV epoxy quaternary ammonium salt to cellulose fiber is 0.1-0.3:1.

[0021] Preferably, Class I epoxy quaternary ammonium salts include epoxy quaternary ammonium salt 1* and epoxy quaternary ammonium salt 2*; Class II, III or IV include epoxy quaternary ammonium salt 3*, epoxy quaternary ammonium salt 4* and epoxy quaternary ammonium salt 5*.

[0022] Preferably, the heating rate in step S2 is 1-3°C / min.

[0023] The invention provides a cationic modifier, comprising a combination of a type I epoxy quaternary ammonium salt and one of type II, III or IV epoxy quaternary ammonium salts, wherein the mass ratio of the type I epoxy quaternary ammonium salt to the cellulose fiber is 0.06-0.1:1; and the type I epoxy quaternary ammonium salt comprises epoxy quaternary ammonium salt 1* and epoxy quaternary ammonium salt 2*; the mass ratio of the type II, III or IV epoxy quaternary ammonium salt to the cellulose fiber is 0.1-0.3:1, and the type II, III or IV epoxy quaternary ammonium salt comprises epoxy quaternary ammonium salt 3*, epoxy quaternary ammonium salt 4* and epoxy quaternary ammonium salt 5*.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The invention provides a method for synthesizing epoxy quaternary ammonium salt, so that the purity of the product reaches more than 95%, which is conducive to the subsequent modification of cotton fiber; the synthesized epoxy quaternary ammonium salt with multiple reactive groups and long carbon chains has improved reaction activity and directness compared with short carbon chain monoepoxy quaternary ammonium salt, and the utilization rate of cationic modifier is improved; the modified fiber has high dye utilization rate during dyeing, the dyeing rate is nearly 100%, and no inorganic salt needs to be added, which reduces the difficulty and cost of treating polluted wastewater; compared with the modification effect of a single modifier, the fiber dyeing of epoxy quaternary ammonium salt composite modified with long-chain alkyl and short-chain alkyl has a higher color yield, and more importantly, the fiber color after dyeing is darker and the saturation is higher, and the dyeing levelness can also meet the relevant requirements. By controlling the chain length, the epoxy quaternary ammonium salt containing long-chain alkyl and short-chain alkyl can complement each other to a certain extent through composite modification, so that the modifier has good permeability and directness at the same time, and the modification quality and dyeing quality are improved.

[0026] The novel cationic modifier prepared by the present invention can simultaneously improve the dye penetration and apparent depth of the dye, not only realizing the improvement of the dye utilization rate under the condition of no salt addition, but also reducing the dosage of the modifier, improving the color strength and color saturation of the dyed fiber, and better meeting the application requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1This is a CIE coordinate diagram of the dyed fabric sample obtained in Example 5 of the present invention compared with the dyed fabric sample with salt and the one modified by a single auxiliary agent;

[0028] Figure 2 These are digital photos of cotton fiber fabric samples after dyeing according to Example 5 of the present invention and Comparative Examples 2 and 3. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited in any way.

[0030] In the following examples, each numbered compound refers to:

[0031]

[0032] Example 1

[0033] Epoxy quaternary ammonium salt synthesis process:

[0034] In a three-necked flask equipped with a N2 protection device, a reflux condenser and a magnet, 10.6 g of tertiary amine 1 # and 5mL of solvent ethanol, place the three-necked flask in a 25℃ water bath. Start magnetic stirring, and slowly add 6.9g of epichlorohydrin in the constant pressure burette to the three-necked flask, and continue stirring for 0.5h after the addition is complete. Next, heat the system to 40℃ to continue the reaction, and test the conversion rate of the product after 2h and 4h of reaction, and stop the reaction after 6h of reaction.

[0035] Then the solution product obtained by the reaction is subjected to reduced pressure distillation to remove unreacted reactants and solvents, and the purification temperature is controlled at 60°C until the product solution is concentrated into a viscous state. The obtained viscous slurry is the desired monoepoxy quaternary ammonium salt 1*, which is cooled and eluted with anhydrous petroleum ether for 5 times, and then vacuum dried at 40°C for 24 hours to obtain a light yellow powder product.

[0036] Example 2

[0037] Epoxy quaternary ammonium salt synthesis process:

[0038] In a three-necked flask equipped with a N2 protective device, a reflux condenser and a magnet, 12.0 g of tertiary amine 2 # and 5mL of solvent ethanol, place the three-necked flask in a 25℃ water bath. Start magnetic stirring, and slowly add 6.9g of epichlorohydrin in the constant pressure burette to the three-necked flask, and continue stirring for 0.5h after the addition is complete. Next, heat the system to 60℃ to continue the reaction, and test the conversion rate of the product after 2h and 4h of reaction, and stop the reaction after 4h of reaction.

[0039] Then the solution product obtained by the reaction is subjected to reduced pressure distillation to remove unreacted reactants and solvents, and the purification temperature is controlled at 60°C until the product solution is concentrated into a viscous state. The obtained viscous slurry is the desired monoepoxy quaternary ammonium salt 2*, which is cooled and eluted with anhydrous petroleum ether for 5 times, and then vacuum dried at 40°C for 24 hours to obtain a white powder product.

[0040] Example 3

[0041] Epoxy quaternary ammonium salt synthesis process:

[0042] 8.6 g of tertiary amine 4 was added to a three-necked flask equipped with a N2 protection device, a reflux condenser and a magnet. # and 5mL of solvent ethanol, place the three-necked flask in an ice-water bath. Start magnetic stirring, and slowly add 13.8g of epichlorohydrin in the constant pressure burette to the three-necked flask, and continue stirring for 0.5h after the addition is complete. Next, heat the system to 25℃ and continue the reaction. Detect the conversion rate of the product at 2h, 4h and 8h of reaction, and stop the reaction after 8h.

[0043] Then the solution product obtained by the reaction is subjected to reduced pressure distillation to remove unreacted reactants and solvents, and the purification temperature is controlled at 60°C until the product solution is concentrated into a viscous state. The obtained viscous slurry is the desired diepoxy quaternary ammonium salt 4*, and after cooling, a yellow powder product is collected.

[0044] Example 4

[0045] Epoxy quaternary ammonium salt synthesis process:

[0046] 8.6 g of tertiary amine 5 was added to a three-necked flask equipped with a N2 protection device, a reflux condenser and a magnet. # and 5mL of methanol solvent, put the three-necked flask into an ice-water bath. Start magnetic stirring, and slowly add 20.8g of epichlorohydrin in the constant pressure burette to the three-necked flask, and continue stirring for 0.5h after the addition is complete. Next, heat the system to 35℃ and continue the reaction. Detect the conversion rate of the product at 2h and 4h of reaction, and stop the reaction after 7h of reaction.

[0047] Then the solution product obtained by the reaction is subjected to reduced pressure distillation to remove unreacted reactants and solvents, and the purification temperature is controlled at 60°C until the product solution is concentrated into a viscous state. The obtained viscous slurry is the desired triepoxy quaternary ammonium salt 5*, and after cooling, a yellow powder product is collected.

[0048] Example 5

[0049] Fiber composite modification and dyeing process:

[0050] Add 0.5g of epoxy quaternary ammonium salt 3*, 0.2g of epoxy quaternary ammonium salt 2* and 15mL of tap water to the container, and then put 5g of wet cotton fiber into the container. Put the sealed container into 30℃ water for reaction for 30min, then add 0.1g of sodium hydroxide to dissolve and heat to 60℃ at a rate of 2℃ / min and continue to react for 30min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of cotton fabric.

[0051] (1) The modified fiber was placed in a reactive brilliant blue KN-R dye bath with a chroma of 3% (owf) and a bath ratio of 1:20. The dyeing was first performed at 30°C for 30 min, then the temperature was raised to 60°C at a rate of 2°C / min and the dyeing was continued for 30 min. The dyed fabric sample was then taken out, washed with water, soaped with a soap solution with a mass fraction of 2‰ using standard soap flakes, with a bath ratio of 1:50, washed again with water, and dried.

[0052] (2) The test results show that the composite modified dyeing has better dyeing levelness than the salt dyeing and the single modifier modified dyeing, and the K / S value is increased by 64.67% and 15.50% respectively. Figure 1 It can be seen that the CIE coordinate diagram shows that the fiber color is darker and has a higher saturation after composite modification and dyeing.

[0053] Comparative Example 1

[0054] Fiber salt dyeing process:

[0055] 5g of soaked fiber was placed in a reactive brilliant blue KN-R dye bath with a color of 3% (owf) and 60g / L sodium sulfate, with a bath ratio of 1:20. It was first dyed at 30℃ for 30min, then heated to 60℃ at a rate of 2℃ / min, and then 10g / L of sodium carbonate was added, and dyeing continued for 30min. Then the dyed fabric sample was taken out, washed with water, soaped with a standard soap flake configuration with a mass fraction of 2‰, with a bath ratio of 1:50, washed again with water, and dried.

[0056] Comparative Example 2

[0057] Fiber single modification and dyeing process:

[0058] (1) Add 0.8 g of epoxy quaternary ammonium salt 3* and 15 mL of tap water to a container, then place 5 g of wet cotton fiber into the container. Place the sealed container in 30°C water for reaction for 30 min, then add 0.15 g of sodium hydroxide to dissolve and heat to 60°C at a rate of 2°C / min and continue to react for 30 min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of the cotton fabric.

[0059] (2) The modified fiber was placed in a reactive brilliant blue KN-R dye bath with a chroma of 3% (owf) and a bath ratio of 1:20. The dyeing was first performed at 30°C for 30 min, then the temperature was raised to 60°C at a rate of 2°C / min and the dyeing was continued for 30 min. The dyed fabric sample was then taken out, washed with water, soaped with a soap solution having a mass fraction of 2‰ using standard soap flakes and a bath ratio of 1:50, and then washed with water and dried.

[0060] Comparative Example 3

[0061] Fiber single modification and dyeing process:

[0062] (1) Add 0.5 g of epoxy quaternary ammonium salt 2* and 15 mL of tap water to a container, and then place 5 g of wet cotton fiber into the container. Place the sealed container in 30°C water for reaction for 30 min, then add 0.15 g of sodium hydroxide to dissolve and heat to 60°C at a rate of 2°C / min and continue to react for 30 min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of the cotton fabric.

[0063] (2) The modified fiber was placed in a reactive brilliant blue KN-R dye bath with a chroma of 3% (owf) and a bath ratio of 1:20. The dyeing was first performed at 30°C for 30 min, then the temperature was raised to 60°C at a rate of 2°C / min and the dyeing was continued for 30 min. The dyed fabric sample was then taken out, washed with water, soaped with a soap solution having a mass fraction of 2‰ using standard soap flakes and a bath ratio of 1:50, and then washed with water and dried.

[0064] Example 6

[0065] Fiber composite modification and dyeing process:

[0066] (1) Add 0.5 g of epoxy quaternary ammonium salt 4*, 0.2 g of epoxy quaternary ammonium salt 2* and 15 mL of tap water to a container, and then place 5 g of wet cotton fiber into the container. Place the sealed container in 30°C water for 20 min, then add 0.1 g of sodium hydroxide to dissolve and heat to 70°C at a rate of 2°C / min to continue the reaction for 20 min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of the cotton fabric.

[0067] (2) The dyeing process is the same as that of Example 5.

[0068] (3) The test results show that the composite modified dyeing has better dyeing levelness than salt dyeing and single modifier modification, and the K / S values ​​are increased by 54.47% and 13.23% respectively. Moreover, the fiber color is darker and the saturation is higher after dyeing.

[0069] Comparative Example 4

[0070] Fiber single modification and dyeing process:

[0071] (1) Add 0.8 g of epoxy quaternary ammonium salt 4* and 15 mL of tap water to a container, and then place 5 g of wet cotton fiber into the container. Place the sealed container in 30°C water for reaction for 30 min, then add 0.15 g of sodium hydroxide to dissolve and heat to 60°C at a rate of 2°C / min to continue the reaction for 30 min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of the cotton fabric.

[0072] (2) The modified fiber was placed in a reactive brilliant blue KN-R dye bath with a chroma of 3% (owf) and a bath ratio of 1:20. The dyeing was first performed at 30°C for 30 min, then the temperature was raised to 60°C at a rate of 2°C / min and the dyeing was continued for 30 min. The dyed fabric sample was then taken out, washed with water, soaped with a soap solution having a mass fraction of 2‰ using standard soap flakes and a bath ratio of 1:50, and then washed with water and dried.

[0073] Example 7

[0074] Fiber composite modification and dyeing process:

[0075] (1) Add 0.5 g of epoxy quaternary ammonium salt 5*, 0.2 g of epoxy quaternary ammonium salt 1* and 15 mL of tap water to a container, and then place 5 g of wet cotton fiber into the container. Place the sealed container in 30°C water for 15 min, then add 0.35 g of sodium hydroxide to dissolve and heat to 80°C at a rate of 2°C / min to continue the reaction for 15 min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of the cotton fabric.

[0076] (2) The modified fiber was placed in a reactive brilliant blue KN-R dye bath with a chroma of 3% (owf) and a bath ratio of 1:10. The dyeing was first performed at 30°C for 30 min, then the temperature was raised to 60°C at a rate of 2°C / min and the dyeing was continued for 30 min. The dyed fabric sample was then taken out, washed with water, soaped with a soap solution having a mass fraction of 2‰ using standard soap flakes and a bath ratio of 1:50, and then washed with water and dried.

[0077] (3) The test results show that the composite modified dyeing has better dyeing levelness than salt dyeing and single modifier modification, and the K / S values ​​are increased by 52.72% and 7.47% respectively. After dyeing, the fiber color is darker and the saturation is higher.

[0078] Comparative Example 5

[0079] Fiber single modification and dyeing process:

[0080] (1) Add 1.5 g of epoxy quaternary ammonium salt 5* and 15 mL of tap water to a container, then place 5 g of wet cotton fiber into the container. Place the sealed container in 30°C water for 30 min, then add 0.15 g of sodium hydroxide to dissolve and heat to 60°C at a rate of 2°C / min to continue the reaction for 30 min. After the reaction is completed, take out the cotton fiber and wash it 1-2 times to complete the cellulose modification process of the cotton fabric.

[0081] (2) The modified fiber was placed in a reactive brilliant blue KN-R dye bath with a chroma of 3% (owf) and a bath ratio of 1:20. The dyeing was first performed at 30°C for 30 min, then the temperature was raised to 60°C at a rate of 2°C / min and the dyeing was continued for 30 min. The dyed fabric sample was then taken out, washed with water, soaped with a soap solution having a mass fraction of 2‰ using standard soap flakes and a bath ratio of 1:50, and then washed with water and dried.

[0082] Example 8

[0083] Fiber composite modification and dyeing process:

[0084] The fiber modification and dyeing process is the same as that in Example 5, but the epoxy quaternary ammonium salts used are 3* and 1*.

[0085] Example 9

[0086] Fiber composite modification and dyeing process:

[0087] The fiber modification and dyeing process are the same as those in Example 6, except that the epoxy quaternary ammonium salts used are 4* and 1*.

[0088] Example 10

[0089] Fiber composite modification and dyeing process:

[0090] The fiber modification and dyeing process are the same as in Example 7, except that the epoxy quaternary ammonium salts used are 5* and 2*.

[0091] Embodiment 11

[0092] The pure cotton fabric was modified and dyed using different modification methods, and the dyeing effects are as follows:

[0093] Table 1. Dyeing effect of different modification methods

[0094]

[0095] The symbols in the table represent: K / S-dyeing depth, L*-brightness, C*-color saturation, h°-hue angle value. The dyeing effect is analyzed, and by comparing the dyeing depth (K / S) and color saturation (C*), it can be found that Example 5 and Example 6 are significantly higher than other examples. Considering comprehensively, Example 5 has the best dyeing effect.

[0096] Color yield, also known as color yield, is a qualitative parameter that indicates the depth of color that a dye can impart to a dyed object. It can be understood as the color depth of a unit weight of dye on a fabric or the amount of dye used to dye 1 / 1 standard depth.

[0097] Conclusion: The above table shows that by comparing the fiber after composite modification with two types of epoxy quaternary ammonium salts with the fiber dyed with salt and dyed with single epoxy quaternary ammonium salt, it can be seen that the composite modified dyeing process has a darker color and the amount of modifier used is reduced. Figure 2 It can be seen that the color of the fabric sample after dyeing with epoxy quaternary ammonium salt 3* alone is darker; the color of the fabric sample after dyeing with epoxy quaternary ammonium salt 2* alone is not uniform but the color is brighter; compared with the single epoxy quaternary ammonium salt modification, the color of the fabric sample after dyeing with epoxy quaternary ammonium salt 2* and 3* modification has the characteristics of uniform color and brighter color. In general, the dyeing of the cationic modified fiber obtained by the composite modification method is improved in terms of dyeing depth and fabric color saturation, and the dyeing effect is good. The composite modification method prepared by the present invention has the advantages of good level dyeing, brighter color and high color depth. The two types of epoxy quaternary ammonium salts used in the present invention play different roles, one type makes the color light brighter and the other type makes the color uniform. Specifically, type I epoxy quaternary ammonium salts are 1* and 2*, which can make the color light bright, and the dosage is 0.06-0.1:1; type II, III, and IV epoxy quaternary ammonium salts are 3*, 4*, and 5*, which make the color uniform, and the dosage is 0.1-0.3:1. Therefore, using more types of epoxy quaternary ammonium salts cannot make it have a better effect.

[0098] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A fiber dyeing method, characterized in that: The following steps are involved: S1, adding the soaked cellulose fiber to an aqueous solution of an epoxy quaternary ammonium salt composition and an alkali agent at a bath ratio of 1:3-5, and then sealing and reacting at 30-40°C, then heating to 60-80°C to continue the reaction, and washing with water to obtain a modified fiber; S2, placing the modified fiber in a dye bath with a chroma of 1-6% (owf) and a bath ratio of 1:5-25, first dyeing at 30-40°C, then heating to 60-70°C, continuing dyeing, washing with water, soaping, bath ratio of 1:50, washing with water again, and drying; The preparation method of the epoxy quaternary ammonium salt comprises: (1) Under nitrogen protection, epichlorohydrin is added dropwise to a tertiary amine dissolved in an organic solvent, mixed evenly at 0-25°C, and heated to 25-60°C to react until the product no longer increases; the tertiary amine is one of formula I, II, III, and IV: Wherein R1 is an alkyl group with a length of 10 to 18, R2 is an alkyl group with a length of 1 to 6, and n is an integer of 2 to 6; (2) Purify and remove impurities, then elute with anhydrous petroleum ether, and then vacuum dry at 30-40°C to obtain the epoxy quaternary ammonium salt corresponding to the tertiary amine of type I, II, III or IV; The epoxy quaternary ammonium salt composition in step S1 includes a Class I epoxy quaternary ammonium salt and one of a Class II, III or IV epoxy quaternary ammonium salt, wherein the mass ratio of the Class I epoxy quaternary ammonium salt to the cellulose fiber is 0.06 to 0.1:1; the mass ratio of the Class II, III or IV epoxy quaternary ammonium salt to the cellulose fiber is 0.1 to 0.3:1; Class I epoxy quaternary ammonium salts include epoxy quaternary ammonium salt 1* and epoxy quaternary ammonium salt 2*; Class II, III or IV include epoxy quaternary ammonium salt 3*, epoxy quaternary ammonium salt 4* and epoxy quaternary ammonium salt 5* respectively; 。 2. The fiber dyeing method according to claim 1, characterized in that: In step S1, the reaction is carried out at 30-40°C for 20-30 min, and the temperature is raised to 60-80°C for further reaction for 10-30 min; in step S2, dyeing is carried out at 30-40°C for 20-30 min, and then the temperature is raised to 60-70°C, and dyeing is continued for 30-40 min; the water washing is performed 1-2 times; and the soap washing includes soap washing with a soap solution having a mass fraction of 2‰ using standard soap flakes.

3. The fiber dyeing method according to claim 1, characterized in that: The organic solvent is one of methanol, ethanol or ethyl acetate; the mass ratio of the organic solvent to epichlorohydrin is 1:2-3.

4. The fiber dyeing method according to claim 1, characterized in that: The purification and impurity removal method comprises distillation under reduced pressure at 60-75°C.

5. The fiber dyeing method according to claim 1, characterized in that: The alkali agent in step S1 includes one or more combinations of sodium hydroxide, potassium hydroxide, sodium carbonate, and potassium carbonate; the mass ratio of the alkali agent to the epoxy quaternary ammonium salt composition is 0.1 to 0.5:

1.

6. The fiber dyeing method according to any one of claims 1-2, characterized in that: The heating rate in step S2 is 1-3°C / min.