Carboxylic acid co-modified polyorganosiloxane and its use

By using linear carboxylic acid co-modified polyorganosiloxane combined with alkaline substances and hydrophilic media, the problem of poor dispersion of hydrophobic powder in the aqueous phase is solved, and the water resistance and sebum resistance of the cosmetic film are achieved. It is suitable for multifunctional cosmetic compositions.

CN116096786BActive Publication Date: 2024-10-18DOW TORAY CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202180062538.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-06
Publication Date
2024-10-18
Estimated Expiration
2041-10-06

AI Technical Summary

Technical Problem

It is difficult to disperse hydrophobic powder stably and uniformly in the water phase with the existing technology, resulting in poor water resistance of the cosmetic film and failure to meet functional requirements such as waterproofness and sebum resistance.

Method used

Linear carboxylic acid co-modified polyorganosiloxane is used as the powder treatment agent. It has a specific carboxyl-containing and silicon-containing organic group structure, which can evenly disperse hydrophobic powder in the water phase and combine with alkaline Substances and hydrophilic media form stable aqueous dispersions.

Benefits of technology

It achieves stable and uniform dispersion of hydrophobic powder in the aqueous phase, provides excellent waterproofing, water resistance and sebum resistance, and is suitable for external use compositions such as cosmetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116096786B_ABST
    Figure CN116096786B_ABST
Patent Text Reader

Abstract

The present invention provides a novel carboxylic acid co-modified polyorganosiloxane, its use as a powder treatment agent, an external preparation composition containing the carboxylic acid co-modified polyorganosiloxane, etc. The carboxylic acid co-modified polyorganosiloxane can stably and uniformly disperse various hydrophobic powders in an aqueous phase and has excellent functions as a powder dispersant, etc. A carboxylic acid co-modified polyorganosiloxane and its use, wherein the carboxylic acid co-modified polyorganosiloxane is represented by the following structural formula (1): {wherein, R 1 is a hydrocarbon group of C6 or less or a hydrogen atom, R 2 is a monovalent hydrocarbon group of C6 to 30, L 1 is a specific organic group containing organosilicon, Rc is an organic group containing carboxyl, and R' is independently selected from the R 1 , R 2 , L 1 As well as the groups in Rc, the molecule must contain Rc and L 1 .}.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carboxylic acid co-modified polyorganosiloxane and its use, in particular to an aqueous powder dispersion (slurry). The carboxylic acid co-modified polyorganosiloxane has a specific carboxyl-containing organic group (hereinafter sometimes referred to as a "carboxylic acid modified group") and a specific silicon-containing organic group in the molecule and is highly useful as a powder treatment agent. Background Art

[0002] Cosmetics containing an aqueous phase as a continuous phase give a moist and refreshing feeling when used, and are therefore widely used in base cosmetics such as emulsions, base makeup cosmetics, sunscreens, foundations, eye shadows, and other makeup cosmetics. In particular, oil-in-water emulsified cosmetics containing inorganic UV-blocking agents represented by hydrophobized microparticles of titanium oxide and hydrophobized microparticles of zinc oxide can be designed to have a high SPF (=Sun Protection Factor) value, which is an indicator of the degree of effect of blocking UV-B waves (wavelength 280 to 315 nm) in ultraviolet rays, and are widely used in sunscreen cosmetics such as sunscreens.

[0003] On the other hand, water-in-oil emulsified cosmetics usually have the problem that the cosmetic film obtained by applying the cosmetic is poor in water resistance. For the purpose of imparting water resistance to the cosmetic film, Patent Documents 1 and 2 propose that carboxylic acid-modified silicones are used under alkaline conditions in order to disperse hydrophobic powders well in the aqueous phase to stabilize the cosmetics or to make aqueous slurries that serve as raw materials for cosmetics. In particular, Patent Document 2 proposes carboxylic acid-modified silicones that optionally have siloxane-modified groups and carboxyl-containing organic groups. However, as for the carboxylic acid-modified silicones specifically proposed in Patent Documents 1 and 2, for some hydrophobic powders such as hydrophobized microparticle zinc oxide, it is sometimes impossible to form a long-term stable aqueous slurry, and the powder dispersibility thereof leaves room for improvement. On the other hand, in Patent Document 3, the applicants of this case proposed that the neutralized salt of modified silicone having a carbosiloxane dendrimer structure and a carboxylic acid modified group be used in an oil-in-water emulsified cosmetic, but did not disclose a linear co-modified siloxane molecule, i.e., a carboxylic acid co-modified polyorganosiloxane having an organic group containing silicone such as a carbosiloxane dendrimer structure in the side chain and a carboxylic acid modified group in the molecule, and also did not record or suggest the use of the neutralized product of the carboxylic acid co-modified polyorganosiloxane as an aqueous dispersant for hydrophobic powders. Similarly, in Patent Document 4, a powder for waterproof cosmetics obtained by treating the powder with a metal cation salt of a carboxylic acid modified polyorganosiloxane is disclosed, but the use of a carboxylic acid co-modified polyorganosiloxane containing a specific organic group containing silicone is also not disclosed. The treated powder is waterproof and does not have dispersibility in an aqueous phase, and therefore cannot solve the technical problem of the present invention.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Patent Publication No. WO2015 / 159773

[0007] Patent Document 2: International Patent Publication No. WO2020 / 036065

[0008] Patent Document 3: International Patent Publication No. WO2009 / 022621

[0009] Patent Document 4: Japanese Patent Application Laid-Open No. 9-59125 Summary of the invention

[0010] Problems to be solved by the invention

[0011] The present invention has been made to solve the above-mentioned problems, and its object is to provide a novel carboxylic acid co-modified polyorganosiloxane which can stably and uniformly disperse various hydrophobic powders in an aqueous phase and has excellent functions as a powder dispersant, etc. Furthermore, it is an object to provide an aqueous powder composition which has excellent workability and can exhibit sufficient functions such as water resistance, water resistance, and sebum resistance when mixed with an external preparation composition such as a cosmetic, and an external preparation composition containing the powder composition by using the carboxylic acid co-modified polyorganosiloxane.

[0012] Solutions for solving problems

[0013] The present inventors have conducted intensive research and have found that the above-mentioned problems can be solved by using the following straight-chain carboxylic acid co-modified polyorganosiloxane, which is liquid at 50° C. and has a carboxyl group in the molecule, thereby achieving the present invention.

[0014] And in the side chain part, there is one or more silicone-containing organic groups (L1) selected from silylalkyl groups having a carbosiloxy dendron structure and groups having a siloxane macromonomer structure at a specific ratio. In addition, it was found that the above-mentioned problems can be solved by using the co-modified polyorganosiloxane as a powder treatment agent, thereby achieving the present invention. Furthermore, it was found that the above-mentioned problems can be solved by the following aqueous powder composition, external preparation composition containing them (especially cosmetics) and the production method thereof, thereby completing the present invention. The aqueous powder composition is made by using the co-modified polyorganosiloxane, an alkaline substance, a hydrophilic medium and a powder to uniformly disperse the powder in the aqueous phase. In particular, when the carboxylic acid co-modified polyorganosiloxane has a specific degree of polymerization described later, etc., and is liquid at room temperature (25°C), the above-mentioned problems can be solved extremely appropriately.

[0015] Beneficial Effects

[0016] According to the present invention, a novel carboxylic acid co-modified polyorganosiloxane can be provided which can stably and uniformly disperse various hydrophobic powders in an aqueous phase and has excellent functions as a powder dispersant, etc. Furthermore, by using the carboxylic acid co-modified polyorganosiloxane as a powder treatment agent, an aqueous powder composition having excellent workability and being able to exhibit sufficient functions such as water resistance, water resistance, and sebum resistance when mixed with an external preparation composition such as a cosmetic can be provided, and an external preparation composition containing the powder composition can be provided. DETAILED DESCRIPTION

[0017] Hereinafter, the co-modified polyorganosiloxane of the present invention, its use as various treatment agents (surfactants or surface treatment agents), particularly its use as a powder treatment agent / powder dispersant, and its use as a cosmetic raw material will be described in detail.

[0018] The carboxylic acid co-modified polyorganosiloxane of the present invention is characterized in that it is liquid at 50°C, is a chain polysiloxane represented by the structural formula (1) described later, has a silicone-containing organic group (L1) selected from a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromonomer structure at its side chain, and has a specific carboxyl-containing organic group in the molecule. The carboxyl-containing organic group in the carboxylic acid co-modified polyorganosiloxane of the present invention can be introduced into the side chain or the terminal, and it is particularly preferred to have the organic group in the side chain. In addition, the carboxylic acid co-modified polyorganosiloxane of the present invention only needs to be liquid at 50°C and 1 atmosphere, for example, it can be solid at room temperature (25°C), but it is particularly preferred to be liquid at room temperature (25°C).

[0019] The carboxylic acid co-modified polyorganosiloxane of the present invention is represented by the following structural formula (1):

[0020] [Chemical formula 1]

[0021]

[0022] In the formula, R 1 is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms or a hydrogen atom, and does not contain other 2 , L 1 The group corresponding to Rc is preferably methyl or phenyl in industry.

[0023] R 2 It is a substituted or unsubstituted linear or branched monovalent hydrocarbon group having 6 to 30 carbon atoms, which may be included arbitrarily in the molecule and may improve the affinity with non-silicone oils such as hydrocarbon oils (cosmetic raw materials). 2 The alkyl group having 6 to 30 carbon atoms includes, for example, hexyl, heptyl, octyl, decyl, dodecyl, undecyl, hexadecyl and the like, and an alkyl group having 8 to 20 carbon atoms is particularly preferred.

[0024] L 1 is a silicon-containing organic group selected from a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromonomer structure, and a specific carboxyl-containing organic group as Rc and at least one L present in the side chain are present at a certain ratio in the molecule of the carboxylic acid co-modified polyorganosiloxane of the present invention. 1 , thereby achieving excellent powder dispersibility, especially in the aqueous phase. More specifically, L in the present invention 1 is one or more groups selected from the following groups,

[0025] When i=1, a silylalkyl group having a siloxane dendron structure represented by the following general formula (2):

[0026] [Chemical formula 2]

[0027]

[0028] (Where R 1 is the same group as above, R C is an alkyl group having 1 to 6 carbon atoms or a phenyl group, and Z is a divalent organic group. i represents L i The number of layers of the silylalkyl group represented by L is an integer of 1 to c when the number of layers as the number of repetitions of the silylalkyl group is c, and the number of layers c is an integer of 1 to 10. i+1 When i is less than c, it is the silylalkyl group; when i=c, it is a methyl group or a phenyl group. i is a number in the range of 0 to 3);

[0029] A chain-like organosiloxane group represented by the following general formula (2'):

[0030] [Chemical formula 3]

[0031]

[0032] (Where R 11 are independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms, a hydroxyl group or a hydrogen atom, and R 11 At least one of them is the monovalent hydrocarbon group. t is a number in the range of 2 to 10, and r is a number in the range of 1 to 500); and

[0033] The chain-like organosiloxane group represented by the following general formula (2"):

[0034] [Chemical formula 4]

[0035]

[0036] (Where R 11 and r as described above).

[0037] L 1 The groups shown may be the same or different. For example, in the same molecule, there may be a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromer structure, a combination of organic groups containing silicone with different branching degrees (generations) in the silylalkyl group, and a combination of organic groups containing silicone with different polymerization degrees in the group having a siloxane macromer structure.

[0038] L 1 The group shown may be a silylalkyl group having a carbosiloxane dendritic macromolecular structure, which is defined as the silylalkyl group shown in the above general formula (2) when i=1. The silylalkyl group having a carbosiloxane dendritic macromolecular structure has a structure in which the carbosiloxane unit is expanded into a dendritic structure, and is therefore a functional group with high water repellency compared to a linear or simple branched polysiloxane unit, without impairing the touch derived from the hydrophilic functional group, and can achieve a high degree of powder dispersibility for the carboxylic acid co-modified polyorganosiloxane of the present application. In addition, the silylalkyl group having a carbosiloxane dendritic macromolecular structure is a functional group that imparts the following advantageous properties: since it is chemically stable, it can be used in combination with a wide range of cosmetic ingredients.

[0039] In the general formula (2), R C It is an alkyl group having 1 to 6 carbon atoms or a phenyl group, and industrially preferably a methyl group or a phenyl group.

[0040] In the general formula (2), i represents L 1The number of layers of the silylalkyl group represented by L is an integer of 1 to c when the number of layers as the number of repetitions of the silylalkyl group is c, and the number of layers c is an integer of 1 to 10. i+1 When i is less than c, it is the silylalkyl group, and when i = c, it is a methyl group or a phenyl group. In particular, when i = c, it is preferably a methyl group.

[0041] The number of layers c is preferably an integer of 1 to 3 in industry, more preferably 1 or

[0042] 2. In each level, the group represented by L1 is as follows. In the formula, R2 and

[0043] Z is the same group as described above.

[0044] When the number of layers c=1, L1 is represented by the following general formula (2-1).

[0045] [Chemical formula 5]

[0046]

[0047] When the number of layers c=2, L1 is represented by the following general formula (2-2).

[0048] [Chemical formula 6]

[0049]

[0050] In formula (2), ai is independently a number in the range of 0 to 3, and in the structures represented by formulas (2-1) to (2-3) when the number of levels is 1 to 3, a1, a2, and a3 are independently a number in the range of 0 to 3. It is particularly preferred that ai is a number in the range of 0 to 1, and ai is particularly preferably 0.

[0051] In the above formula, Z is independently a divalent organic group, specifically, a divalent organic group formed by addition reaction of a silicon-bonded hydrogen atom with a functional group having an unsaturated hydrocarbon group such as an alkenyl group, an acryloyloxy group, or a methacryloyloxy group at the terminal, but it is not limited to these functional groups and can be appropriately selected according to the introduction method of the silylalkyl group having a carbosiloxane dendron structure. Z in the present invention is preferably an alkylene group having 2 to 10 carbon atoms, and most preferably an ethylene group.

[0052] L 1 The group shown may be a group containing a siloxane macromolecular monomer structure bonded to the silicon atom constituting the main chain via oxygen or alkylene, is hydrophobic, and is a functional group with a certain degree of water repellency / lipophilicity, does not damage the touch derived from the hydrophilic functional group, and achieves a high degree of powder dispersibility for the carboxylic acid co-modified polyorganosiloxane of the present application. Specifically, L 1The groups shown can be functional groups shown in the above general formula (2') and general formula (2"), where R 11 Industrially, methyl, phenyl or hydroxyl groups are particularly preferred. 11 A preferred embodiment is one in which a part of R is a methyl group and a part of R is a long-chain alkyl group having 8 to 30 carbon atoms. 11 At least one of them is a monovalent hydrocarbon group such as a methyl group, t is a number in the range of 2 to 10, and r is a number in the range of 1 to 500. From the viewpoint of compatibility with various oils, r is preferably a number in the range of 1 to 100, and particularly preferably a number in the range of 2 to 30.

[0053] Rc is the general formula: -Rc 1 -(ORc 2 )p-(O)w-Rc 3 -COOH-containing organic group (Rc 1 represents a linear or branched alkylene group having 2 to 22 carbon atoms, Rc 2 represents a linear or branched alkylene group having 2 to 4 carbon atoms, Rc 3 represents a bond (-) or a linear or branched alkylene group having 1 to 22 carbon atoms, p represents a number from 0 to 200, and w represents a number of 0 or 1), and L 1 The specific silicon-containing organic group is present in the molecule, and in particular, the neutralization salt of the alkaline substance can achieve excellent powder dispersibility in the aqueous phase.

[0054] In the general formula representing the carboxyl-containing organic group, Rc 1 The alkylene group is a linear or branched group having 2 to 22 carbon atoms, preferably a linear group having 2 to 12 carbon atoms, particularly preferably a linear group having 2 to 10 carbon atoms, and examples thereof include a decamethylene group.

[0055] In addition, as Rc 2 The linear or branched alkylene group having 2 to 4 carbon atoms includes, for example, ethylene, propylene, trimethylene and butylene.

[0056] Rc 3 It may be a bond (-) or a linear or branched alkylene group having 1 to 22 carbon atoms.

[0057] p represents a number of 0 to 200, preferably a number of 0 to 20, and particularly preferably a number of 0 to 10. In addition, w represents a number of 0 or 1, but preferably 0. In the case where both p and w are 0 and Rc 3 In the case of a bonding bond (-), the carboxyl-containing organic group is represented by the structural formula -(C n H 2n)-COOH represents a structure in which one carboxyl group is bonded to a silicon atom via a linear or branched alkylene group. In the formula, n is preferably a number of 3 to 20, and particularly preferably a number of 3 to 16.

[0058] R' is independently selected from the R 1 , R 2 , L 1 And the group in Rc, if R' is L 1 , is a structure having a silicon-containing organic group at the end of the molecular chain, and if R' is Rc, is a structure having a carboxyl-containing organic group at the end of the molecular chain, preferably a methyl group. However, when n4 described later is 0, the carboxylic acid co-modified polyorganosiloxane of the present invention has more than one Rc, so at least one of R' is Rc.

[0059] In the structural formula (1), n1 to n4 representing the average degree of polymerization of each diorganosiloxy unit, (n1+n2+n3+n4) is a number in the range of 1 to 1000, preferably 2 to 50, and particularly preferably 2 to 20. That is, from the viewpoint of powder dispersibility in an aqueous phase, the carboxylic acid co-modified polyorganosiloxane of the present invention is preferably a relatively low polymerization. In particular, in the case of a relatively low polymerization, it is liquid at room temperature (25° C.) and has a low viscosity, and is therefore also advantageous in preparing an aqueous slurry.

[0060] Furthermore, in the structural formula (1), n1 is a number in the range of 0 to 999, more preferably 0 to 49, and most preferably 0 to 5. n2 is a number in the range of 0 to 100, more preferably 0 to 10. n3 is a number in the range of 1 to 100, more preferably 1 to 10. n4 is a number in the range of 0 to 100, more preferably 0 to 10.

[0061] From the viewpoint of the effect of the present invention, n1 to n4 are numbers within the range in which the carboxylic acid co-modified polyorganosiloxane of the present invention is liquid at room temperature (25°C), and it is particularly preferred to be low in viscosity. The carboxylic acid co-modified polyorganosiloxane that is liquid at room temperature (25°C) and has a low viscosity has the advantages of excellent dispersion effect on hydrophobic powders and no need for heating when forming an aqueous dispersion composition.

[0062] From the viewpoint of the effect of the present invention, it is particularly preferred that, in the above structural formula (1), (n1+n2+n3+n4) is a number in the range of 2 to 20, n3 is a number in the range of 1 to 10, n4 is a number in the range of 1 to 10, and (n1+n2+n3) / n4 is in the range of 0.1 to 5.0. The carboxylic acid co-modified polyorganosiloxane having the above structure has L as a side chain in a certain ratio in its molecular chain. 1The structure of the silicon-containing organic group as Rc and the carboxyl-containing organic group as Rc has an excellent powder treatment effect, and the uniform dispersibility of the hydrophobic powder in the water phase is further improved. With this, when the aqueous dispersion composition containing the carboxylic acid co-modified polyorganosiloxane is used as a cosmetic raw material, it has the advantage of being able to effectively achieve sufficient waterproofness, water resistance, sebum resistance and other functions. Furthermore, it has the advantage of being able to maintain the uniform dispersion state of the hydrophobic powder in the water phase for a long time.

[0063] The carboxylic acid co-modified polyorganosiloxane of the present invention can be produced by the following method: after reacting a compound having an organic group containing silicone (for example, the silylalkyl group) having a carbon-carbon double bond at one end of the molecular chain with a polyorganosiloxane having a reactive functional group such as Si—H, an unsaturated carboxylic acid ester compound, an unsaturated carboxylic acid silyl ester or an allyloxycarboxylic acid silyl ester is subjected to an addition reaction in the presence of a platinum catalyst, and the target product is obtained by further saponification or hydrolysis after the reaction.

[0064] [Application of carboxylic acid co-modified polyorganosiloxane]

[0065] The novel carboxylic acid co-modified polyorganosiloxane of the present invention has a highly water-repellent silicon-containing organic group and a hydrophilic carboxyl-containing organic group in the same molecule and preferably has a low viscosity, so it is excellent in operability, work efficiency, and stability in combination with various cosmetic raw materials. Therefore, it is useful as various treatment agents and cosmetic raw material components, and is particularly useful as a powder surface treatment agent, surfactant or powder dispersant used for surface treatment of hydrophobic powders used in cosmetics and dispersion of powders in an aqueous phase.

[0066] [Use as powder treatment agent or powder dispersant]

[0067] The carboxylic acid co-modified polyorganosiloxane of the present invention functions as a surface treatment agent or dispersant for powders, particularly hydrophobic powders, and can form an aqueous powder composition in which the hydrophobic powder is uniformly and stably dispersed in an aqueous phase by preferably using it in combination with an alkaline substance for hydrophobic powders. In particular, the carboxylic acid co-modified polyorganosiloxane composition containing (A) the carboxylic acid co-modified polyorganosiloxane of the present invention, (B) an alkaline compound, and (C) a hydrophilic medium selected from one or more of water, polyols, and lower alcohols forms a carboxylate structure in which the carboxylic acid residues are partially neutralized in the hydrophilic medium, and is therefore particularly useful as a powder surface treatment agent, surfactant, or surface treatment agent as a dispersant for hydrophobic powders.

[0068] 〔Powder composition〕

[0069] The present invention relates to a powder composition comprising: (A) the carboxylic acid co-modified polyorganosiloxane of the present invention, (B) a basic compound, (C) one or more hydrophilic media selected from water, polyols and lower alcohols, and (D) a powder or a colorant. The powder composition preferably comprises (D1) a hydrophobic powder or a colorant, and has a structure in which the component (D1) is dispersed in an aqueous phase. The powder composition containing the carboxylic acid co-modified polyorganosiloxane of the present invention can be suitably used as an external preparation composition, particularly a cosmetic or a cosmetic raw material.

[0070] The powder composition of the present invention is preferably an aqueous dispersion composition having an aqueous phase composed of a hydrophilic medium as a continuous layer, and is a composition in which a powder or a colorant, particularly a hydrophobic powder or a colorant, is dispersed in a hydrophilic medium. It usually has fluidity, and is therefore sometimes referred to as a "water-based slurry". It should be noted that the hydrophilic medium in the present invention refers to an aqueous dispersion medium containing one or more alcohols selected from water, polyols, ethanol and other lower alcohols that can be uniformly mixed with water, and salts such as alkaline substances. It is particularly preferred that the hydrophilic medium substantially does not contain an oil agent or an oily cosmetic raw material that does not mix with water and can form an independent oil phase.

[0071] It should be noted that the carboxylic acid co-modified polyorganosiloxane of the present invention can be used in the same manner as the carboxylic acid-modified silicone specifically disclosed in the above-mentioned Patent Document 1 or Patent Document 2. On the other hand, it is useful from the perspective of being able to easily prepare an aqueous slurry with low viscosity and excellent long-term storage stability even when these conventionally known carboxylic acid-modified silicones are inorganic powders such as zinc oxide that cannot be fully processed.

[0072] [(B) Alkaline substances]

[0073] The powder composition of the present invention preferably contains at least one (B) alkaline substance. Component (B) can anionize the carboxylic acid modified site of the carboxylic acid co-modified polyorganosiloxane of the present invention (A), thereby improving its function as a surfactant / powder dispersant. In particular, the aqueous dispersion composition of the present invention contains (D) powder or colorant, preferably (D1) hydrophobic powder or colorant, but by using the components (A) and (B) together, the component (D) can be well dispersed in the aqueous phase compared to using the component (A) alone, which not only improves the uniform dispersibility and stability of the aqueous dispersion composition, but also helps to achieve sufficient waterproofness, water resistance, and sebum resistance in the cosmetics formed by combining the aqueous dispersion composition as a cosmetic raw material.

[0074] The alkaline substance used in the present invention is not particularly limited as long as it is a compound that shows alkalinity when dissolved in water, and various inorganic compounds and organic compounds can be used. One or more alkaline substances may be mixed.

[0075] Examples of the organic compound include monoethanolamine, triethanolamine, 2-amino-2-methyl-1,3-propanediol, aminomethylpropanol, aminomethylpropanol, 2-amino-2-hydroxymethyl-1,3-propanediol, arginine, and guanidine.

[0076] Examples of the inorganic compound include sodium hydroxide, sodium carbonate, potassium hydroxide, potassium carbonate, calcium hydroxide, calcium carbonate, and ammonia. Among them, potassium hydroxide can be particularly preferably used.

[0077] The amount of the basic compound in the aqueous dispersion composition of the present invention is not particularly limited, but in the case of a monobasic base, the carboxylic acid group / monobasic base (molar ratio) is preferably 1 / 0.5 to 1 / 1.5 relative to 1 mol of the carboxylic acid group contained in the (A) carboxylic acid co-modified polyorganosiloxane.

[0078] The pH of the aqueous dispersion composition of the present invention may be acidic or alkaline, but from the viewpoint of anionizing the carboxylic acid modified site of the (A) carboxylic acid co-modified polyorganosiloxane and improving the dispersibility with respect to the powder or colorant as component (D), the pH of the aqueous dispersion composition is preferably weakly acidic to alkaline. Specifically, the pH of the composition as a whole is preferably in the range of 6.5 to 14.0, may be in the range of pH 7.1 to 10.0, and more preferably in the range of 7.2 to 9.5.

[0079] [(C) Hydrophilic medium]

[0080] The hydrophilic medium is the main dispersion medium of the powder composition of the present invention, and is one or more selected from water, polyols and lower alcohols, and forms the aqueous phase of the composition. The powder composition of the present invention is preferably an aqueous dispersion, and in the presence of the components (A) and (B), preferably forms a structure in which the powder or colorant as the component (D) is stably dispersed in the aqueous phase.

[0081] The hydrophilic medium of the present invention preferably contains water. On the other hand, the carboxylic acid co-modified polyorganosiloxane (A) has a silicon-containing organic group and a carboxyl-containing organic group in the same molecule that exhibit high water repellency, and therefore, unlike conventionally known carboxylic acid-modified silicones, can sometimes form an aqueous dispersion composition having excellent uniform dispersibility and stability of the powder or colorant as component (D) in the aqueous phase even when it does not contain one selected from polyols and lower alcohols (particularly ethanol).

[0082] When the hydrophilic medium of the present invention contains a polyol and a lower alcohol (particularly ethanol), the powder or colorant as component (D) may also be excellent in uniform dispersibility and stability in the aqueous phase, and when the aqueous dispersion composition of the present invention is used as a raw material for cosmetics, the moisturizing feeling and the feeling during use can be adjusted. In particular, when used as a raw material for cosmetics, the hydrophilic medium as component (C) in the powder composition preferably contains water, but component (C) may also be a mixture containing one or more selected from (C1) water, (C2) polyols and lower alcohols (preferably ethanol).

[0083] As polyols, for example, sorbitol, xylitol, propylene glycol, dipropylene glycol, 1,3-butylene glycol, glycerol, diglycerol, polyethylene glycol, etc. can be listed, and these polyols can be used alone or in combination of two or more. On the other hand, lower alcohols are represented by methanol and ethanol, but from the viewpoint of use as a raw material for cosmetics, non-toxic ethanol is particularly preferred. Lower alcohols can be used alone or in combination with the polyols. Specifically, ethanol and the polyols can be mixed in any mass ratio of 100:0 to 0:100 or used alone in the present invention, and at this time, water may be further included or may not be included.

[0084] 〔(D) Powder or colorant〕

[0085] The (D) powder or colorant used in the powder composition (especially aqueous slurry) of the present invention is a substance generally used as a component of cosmetics, including white and coloring pigments and extender pigments. White and coloring pigments are used for coloring cosmetics, etc., while extender pigments are used for improving the touch of cosmetics, etc. As the "powder" of the present invention, white and coloring pigments and extender pigments commonly used in cosmetics can be used without particular restrictions. In the present invention, it is preferred to mix one or more powders. There is no limitation on the shape (spherical, rod-shaped, needle-shaped, plate-shaped, irregular, spindle-shaped, cocoon-shaped, etc.), particle size (smoke-shaped, microparticles, pigment grade, etc.), and particle structure (porous, non-porous, etc.) of the powder, and the average primary particle size is preferably in the range of 1nm to 100μm. In particular, when these powders or colorants are used as pigments, it is preferred to mix one or more selected from inorganic pigment powders, organic pigment powders, and resin powders with an average particle size in the range of 1nm to 20μm.

[0086] As powder, for example, inorganic powder, organic powder, surfactant metal salt powder (metal soap), colored pigment, pearlescent pigment, metal powder pigment, etc. can be listed, and these composite powders can be used. Powders whose surfaces are hydrophobized or waterproofed can be further listed. In particular, in the present invention, the preferred component (D) is a hydrophobic powder or colorant (D1) treated with hydrophobicity. The specific examples of hydrophobic treatment and hydrophobic powder are the same as the hydrophobic powder or colorant disclosed in paragraphs 0043 to 0054 of the above-mentioned patent document 2 (International Publication Patent WO2020 / 036065 Gazette) by the applicant, etc.

[0087] Hydrophobic powders are difficult to disperse in an aqueous phase because their surfaces are hydrophobized. However, by using the carboxylic acid co-modified polyorganosiloxane of the present invention, a composition (including use as a cosmetic raw material or an external preparation composition) in which a large amount of hydrophobic powders or colorants are uniformly and stably dispersed in an aqueous phase can be achieved. This has the advantage that even inorganic powders such as zinc oxide, which cannot be sufficiently dispersed under the same conditions as conventional carboxylic acid-modified silicones, can be prepared into an aqueous slurry with a low viscosity.

[0088] Preferably, as the hydrophobic powder used in the present invention, titanium oxide, zinc oxide, iron oxide, cerium oxide and their composites with ultraviolet absorption / scattering ability are preferably used as inorganic powders with hydrophobic surface treatment, and the composites are powders in which other inorganic particles are dispersed inside the surface-treated powders and inorganic powders. Particularly preferred is (D1-1) hydrophobicized microparticles of titanium oxide or hydrophobicized microparticles of zinc oxide with an average particle diameter in the range of 1 to 200 nm, and by using the carboxylic acid co-modified polyorganosiloxane of the present invention preferably together with the above-mentioned components (B) and (C), a powder composition, especially an aqueous dispersion composition, in which these powders or colorants are uniformly and stably dispersed in an aqueous phase is formed.

[0089] [Powder composition as raw material for cosmetics, etc. and its composition]

[0090] The powder composition of the present invention comprising a carboxylic acid co-modified polysiloxane and a powder or a colorant is preferably an aqueous dispersion composition in which an aqueous phase composed of a hydrophilic medium is provided as a continuous layer. It is a composition in which a powder or a colorant, particularly a hydrophobic powder or a colorant, is dispersed in a hydrophilic medium, and can be used as a raw material used in a composition of cosmetics / paints / inks, etc. (hereinafter referred to as "cosmetics, etc.").

[0091] When used as a raw material for cosmetics, the content of the above-mentioned components (A) to (D) is preferably 80% by mass or more, more preferably 90% by mass or more, relative to the total amount of the composition. Furthermore, the powder composition of the present invention can form a low-viscosity aqueous slurry even if it contains a relatively large amount of powder or colorant. Therefore, the powder or colorant as component (D), preferably (D1) hydrophobic powder or colorant, is contained in the range of 10 to 70% by mass of the entire composition, preferably in the range of 15 to 65% by mass, and more preferably in the range of 15 to 60% by mass, so that the powder or colorant is uniformly and stably dispersed in the aqueous phase.

[0092] When used as a raw material for cosmetics, etc., the component (A) in the powder composition is preferably contained in the range of 5 to 30 parts by mass, and more preferably in the range of 10 to 25 parts by mass, relative to 100 parts by mass of the component (D), especially the (D1) hydrophobic powder or colorant. When the amount of the component (A) is less than the lower limit, the dispersion of the hydrophobic powder or colorant in the aqueous phase may become insufficient, and when the amount of the component (A) exceeds the upper limit, the component (D) may not be mixed in a sufficient amount in the powder composition as an aqueous slurry.

[0093] When used as a raw material for cosmetics, the hydrophilic medium as component (C) in the powder composition preferably includes water. Specifically, when component (C) includes one or more selected from (C1) water and (C2) polyols and lower alcohols (preferably ethanol), the content of component (C1) is preferably in the range of 10 to 80% by mass, more preferably 15 to 70% by mass, and particularly preferably 20 to 65% by mass, based on the total mass of the powder composition. In addition, component (C2) is preferably in the range of 0.1 to 50% by mass, more preferably 0.5 to 45% by mass, further more preferably 1 to 40% by mass, and particularly preferably 2 to 35% by mass, based on the total mass of the powder composition.

[0094] When used as a raw material for cosmetics, the powder composition of the present invention preferably does not contain components other than the above components in a ratio exceeding 20% ​​by mass of the whole, and may contain other components in a ratio of 10% by mass or less within a range that does not impair the performance of the dispersion. However, it is preferred not to add compounds that may impair the stability of the dispersion. In particular, the addition of an oil is not preferred.

[0095] As the components that can be added arbitrarily, there is no particular limitation, and preservatives can be listed. Yes. That is, the aqueous dispersion composition composed of the above-mentioned components sometimes becomes corrupt due to the storage conditions and storage period. In order to prevent such corruption, a preservative can also be added. Such preservatives are not particularly limited, for example, glycol preservatives such as propylene glycol, butylene glycol, dipropylene glycol, pentylene glycol, hexylene glycol, benzoic acid esters such as methyl paraben, pyridone ethanolamine salt (piroctone olamine), phenoxyethanol, polyglycerol-3 caprylate, etc. can be listed. They exert antiseptic properties according to the ingredients, and can be added within the range that does not adversely affect the performance of the carboxylic acid co-modified polyorganosiloxane as a dispersant. Among them, pentylene glycol and 1,3-butanediol are particularly preferably used. From the above-mentioned application point of view, the components other than the carboxylic acid co-modified polyorganosiloxane, powder or colorant, water, and preservative of the present invention are preferably set to 1% or less. Among them, the above-mentioned diols are often used as moisturizers in cosmetics, but they also have an effect as a preservative due to their antibacterial properties.

[0096] These components are components that overlap with part of the above-mentioned component (C). Therefore, by using a polyol as component (C), even without adding a preservative, a humectant, etc. separately, the storage stability and the moisturizing function of the powder composition of the present invention, especially the aqueous slurry, can sometimes be improved.

[0097] There are no particular restrictions on the dispersion method for obtaining the powder composition of the present invention, especially a composition in which a powder or a colorant is dispersed in a hydrophilic medium, as long as it is a known method that can uniformly disperse the components using mechanical force. Preferably, a method using a bead mill, a method using a high-pressure homogenizer, a method using three rolls, etc. are used.

[0098] The powder composition obtained in the present invention can also be applied to make a film. For example, by applying a zinc oxide dispersion treated with silicone and heat-treating it at high temperature, plasma, etc., a zinc oxide coating fixed with silicon dioxide can be made. In addition, when a dispersant such as polyether or polyether alkyl ether is used as a dispersant in the same zinc oxide dispersion, a silicone-coated zinc oxide coating can be easily made by heating at a temperature lower than the decomposition temperature of the silicone coated with zinc oxide. It should be noted that, needless to say, other powders can also form a coating.

[0099] [Uses of aqueous dispersion composition: cosmetic raw materials, etc.]

[0100] In addition, the aqueous dispersion composition of the present invention can also be directly mixed with cosmetics, coatings, and inks. In this case, the cosmetic composition, aqueous coating, and ink composition can be obtained by mixing the dispersion with various components used in cosmetics, coatings, and inks. In particular, the aqueous dispersion composition of the present invention is preferably used as a cosmetic raw material directly mixed with cosmetics.

[0101] The cosmetics thus obtained can appropriately disperse the hydrophobic powder in the aqueous phase of the aqueous composition or emulsion, so that the cosmetics prepared by blending the aqueous dispersion can obtain sufficient functions such as water resistance, water resistance, and sebum resistance.

[0102] The cosmetics are not particularly limited, and by mixing cosmetic raw materials into the aqueous dispersion composition of the present invention as needed, it is possible to obtain UV protection cosmetics such as sunscreens, base makeup cosmetics such as foundations, and point makeup cosmetics such as lipsticks. That is, the aqueous dispersion composition of the present invention can be directly used for the manufacture of cosmetics.

[0103] The cosmetics can be in any form of oily cosmetics, water-based cosmetics, O / W cosmetics, or W / O cosmetics. In particular, since inorganic UV-blocking agents can be incorporated in large amounts and stably, they can be particularly suitably used in sunscreen cosmetics (including sunscreens).

[0104] The above-mentioned cosmetics may also be used in combination with any aqueous component or oily component that can be used in the cosmetics field. The above-mentioned aqueous component and oily component are not particularly limited, and may contain, for example, oils, surfactants, humectants, higher alcohols, metal chelating agents, natural and synthetic polymers, water-soluble and oil-soluble polymers, ultraviolet shielding agents, various extracts, colorants such as organic dyes, preservatives, antioxidants, pigments, thickeners, pH adjusters, fragrances, cooling agents, antiperspirants, bactericides, skin activators, various powders and other ingredients.

[0105] As these components, for example, the components specifically disclosed in Patent Document 1 and Patent Document 2 mentioned above can be used without limitation.

[0106] When the aqueous dispersion composition of the present invention is added to a coating, the resin in the coating may or may not be curable. The coating may be a solvent-based coating containing an organic solvent or a water-based coating in which the resin is dissolved or dispersed in water.

[0107] When the aqueous dispersion composition of the present invention is used as an additive to a coating composition, it can be used together with a coating film-forming resin such as an acrylic resin, a polyester resin, an epoxy resin, a coloring pigment, a body pigment, a bright pigment, and other pigments, a curing catalyst, a surface conditioner, a defoaming agent, a pigment dispersant, a plasticizer, a film-forming aid, an ultraviolet absorber, an antioxidant, and the like.

[0108] Furthermore, the aqueous coating material and aqueous ink composition thus obtained are preferred in that the hydrophobic powder is stably dispersed in the aqueous medium.

[0109] [External application composition]

[0110] As described above, the carboxylic acid co-modified polyorganosiloxane and the composition containing the carboxylic acid co-modified polyorganosiloxane of the present invention can be used as a cosmetic raw material in combination with an external-use agent composition. Such an external-use agent composition can contain the above-mentioned carboxylic acid co-modified polyorganosiloxane (=component (A)), can contain a carboxylic acid co-modified polyorganosiloxane composition containing the above-mentioned components (A), (B) and (C) and having a structure in which the carboxylic acid-modified group is partially neutralized in a hydrophilic medium, and can contain a carboxylic acid co-modified polyorganosiloxane composition containing the above-mentioned components (A), (B), (C) and (D) and having a structure in which the component (D) as a powder or a colorant is dispersed in a hydrophilic medium.

[0111] It is particularly preferred that the topical composition of the present invention comprises the above-mentioned components (A), (B), (C) and (D), and preferably has a structure in which the component (D) as a powder or colorant is dispersed in the aqueous phase. As described above, by using the carboxylic acid co-modified polyorganosiloxane of the present invention, the hydrophobic powder or colorant (D1) can be stably dispersed in the aqueous phase, and in particular, the hydrophobic microparticle titanium oxide or hydrophobic microparticle zinc oxide (D1-1) useful as an inorganic UV-blocking agent with an average particle diameter of 1 to 200 nm can be stably and uniformly dispersed in the aqueous phase in large quantities, thereby providing a topical composition having high storage stability and UV protection performance, and not damaging its touch, feel of use, and excellent water resistance of the film (cosmetic film). In particular, it can be expected that by utilizing the carboxylic acid co-modified polyorganosiloxane of the present invention, the degree of freedom of formula design can be further improved, and sunscreen cosmetics having both performances such as water resistance, feel of use, and UV protection represented by SPF values ​​can be provided.

[0112] The topical composition of the present invention is not particularly limited as long as it is a composition applied to the human body as a cosmetic or medicine. As for the cosmetic of the present invention, as specific products, examples can be shown: skin cleanser products, skin care products, makeup products, antiperspirant products, UV protection products and other skin cosmetics; hair cleanser products, hair tidying products, hair dyeing products, hair nourishing products, hair care products (Hair rinse products), hair conditioner products (Hairconditioner products), hair care products (Hair treatment products) and other hair cosmetics; bath cosmetics. The medicine of the present invention can be exemplified by hair growth agents, hair care agents, analgesics, bactericides, anti-inflammatory agents, cooling agents, skin anti-aging agents, but are not limited thereto.

[0113] The topical composition of the present invention can and preferably further include carboxylic acid-modified silicones other than oily agents, the above-mentioned component (A), salts of higher fatty acids, various surfactants (can be selected from one or more of anionic, cationic, nonionic, amphoteric, and can be cleaning agent components), water-soluble tackifiers, oil-soluble film-forming agents, water-soluble ultraviolet absorbers, and vinyl polymer emulsions. It should be noted that the specific examples of these components, in addition to the above-mentioned patent document 1 (WO2015 / 159773 publication), can also be the same components as those proposed by the applicant in the international patent application (PCT / JP19 / 029957). In addition, by using these components (for example, vinyl polymer emulsions) in combination, it is possible to achieve the effect of further improving the dispersibility of powders, etc. in the aqueous phase and improving the SPF value of the overall cosmetic.

[0114] In the external preparation composition of the present invention, other ingredients commonly used in cosmetics may be added within the range that does not hinder the effect of the present invention: for example, hydrophilic powder, moisturizers other than component (C), gelling agents, preservatives, antibacterial agents, fragrances, salts, antioxidants, pH adjusters other than component (B), chelating agents, cooling agents, anti-inflammatory agents, physiologically active ingredients (whitening agents, cell activators, rough skin improvers, blood circulation promoters, skin tightening agents, anti-seborrheic agents, etc.), vitamins, amino acids, nucleic acids, hormones, inclusion compounds, etc. Other ingredients are not particularly limited.

[0115] [Common uses and substitutions with conventional carboxylic acid-modified silicones, especially commercial products]

[0116] The carboxylic acid co-modified polyorganosiloxane of the present invention can be used for the same purpose as carboxylic acid-modified silicone in cosmetics proposed by the applicant of the present case in the above-mentioned Patent Document 1 (International Patent Publication No. WO2015 / 159773) and Patent Document 2 (International Patent Publication No. WO2020 / 036065), and can be used to replace part or all of the carboxylic acid-modified silicone. Similarly, the carboxylic acid co-modified polyorganosiloxane of the present invention can be used in the cosmetics proposed by the applicant of this case in international patent applications (PCT / JP19 / 029957, PCT / JP19 / 029927), international patent publications WO / 2020 / 036064, international patent publications WO / 2020 / 036061, international patent publications WO / 2020 / 036062, and international patent publications WO / 2020 / 036063 for the same purpose as the carboxylic acid-modified silicone in the formulation, and can be used to replace part or all of it. Sometimes, without impairing the advantageous technical effects, feel in use, and touch of these cosmetics containing carboxylic acid-modified silicones, the uniform dispersibility and storage stability of the hydrophobic powder or colorant in the formulation can be further improved.

[0117] Furthermore, the carboxylic acid co-modified polyorganosiloxane of the present invention can be used for the same purpose as the carboxylic acid-modified silicone product marketed by the applicant of the present case as the trade name ES-5800 Formulation Aid (manufactured by DOW TORAY CO., LTD.). The applicant of the present case explicitly teaches that the carboxylic acid-modified silicone product can be used as a replacement for part or all of the carboxylic acid-modified silicone product in the method of use and formulation of the cosmetics disclosed for the carboxylic acid-modified silicone product.

[0118] Example

[0119] The present invention will be described in further detail below based on examples, but the present invention is not limited to these examples. The amount of each component is expressed as "mass %" ("weight %") unless otherwise specified. In addition, in the structural formula, Me is a methyl group and Bu is a butyl group.

[0120] [Examples 1 to 4]

[0121] The carboxylic acid co-modified polyorganosiloxane (Compounds 1 to 4) of the present invention was synthesized by the following method.

[0122] [Example 1]

[0123] In a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 126.90 g of undecylenic acid trimethylsilyl ester, 78.90 g of tris(trimethylsiloxy)vinylsilane, and 0.025 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 94.20 g of a methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature at 70-80°C.

[0124] [Chemical formula 7]

[0125]

[0126] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 3 hours. The low boiling point components were distilled off under reduced pressure. Then, 45 g of ion exchange water was added and the mixture was aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain compound 1. The results of the analysis confirmed that it was compound 1 shown in the following chemical formula.

[0127] [Chemical formula 8]

[0128]

[0129] [Example 2]

[0130] Into a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer were added 44.54 g of undecylenic acid trimethylsilyl ester, 52.29 g of a macromonomer raw material represented by Bu-(OSiMe2)6-CH=CH2, and 0.018 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, and 33.18 g of a methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature in the range of 70-80°C.

[0131] [Chemical formula 9]

[0132]

[0133] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 3 hours. The low boiling point components were distilled off under reduced pressure. Then, 20 g of ion exchange water was added and the mixture was aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain compound 2. The results of the analysis confirmed that it was compound 2 shown in the following chemical formula.

[0134] [Chemical formula 10]

[0135]

[0136] [Example 3]

[0137] In a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 235.52 g of undecylenic acid trimethylsilyl ester, 45.92 g of tris(trimethylsiloxy)vinylsilane and 0.078 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 68.57 g of methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature in the range of 70 to 80°C.

[0138] [Chemical formula 11]

[0139]

[0140] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 3 hours. The low boiling point components were distilled off under reduced pressure. Then, 90 g of ion exchange water was added and the mixture was aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain compound 3. The results of the analysis confirmed that it was compound 3 shown in the following chemical formula.

[0141] [Chemical formula 12]

[0142]

[0143] [Example 4]

[0144] Into a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 120.58 g of undecylenic acid trimethylsilyl ester, 44.24 g of a macromonomer raw material represented by Bu-(OSiMe2)6-CH=CH2, and 0.044 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 35.18 g of methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature in the range of 70-80°C.

[0145]

[0146] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 3 hours. The low boiling point components were distilled off under reduced pressure. Then, 50 g of ion exchange water was added and the mixture was aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain compound 4. The results of the analysis confirmed that it was compound 4 shown in the following chemical formula.

[0147] [Chemical formula 13]

[0148]

[0149] The carboxylic acid-modified silicones (Comparative Compounds 1 to 3) used in the comparative experiments were synthesized by the following method.

[0150] [Comparative Synthesis Example 1]

[0151] In a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 230.67 g of undecylenic acid trimethylsilyl ester and 0.042 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 129.33 g of methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature at 70-80°C.

[0152] [Chemical formula 14]

[0153]

[0154] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 2 hours. The low boiling point components were distilled off under reduced pressure. Then, 90 g of ion exchange water was added and the mixture was aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain comparative compound 1. The results of the analysis confirmed that it was comparative compound 1 shown in the following chemical structural formula.

[0155] [Chemical formula 15]

[0156]

[0157] [Comparative Synthesis Example 2]

[0158] To a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 100 g of 1,1,1,3,5,5,5-heptamethyltrisiloxane and 0.02 g of a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 105 g of undecylenic acid trimethylsilyl ester was added dropwise while maintaining the temperature in the range of 70-100°C. After the addition was completed, the reaction was confirmed to be complete by a hydrogen generation method after aging at 110°C for 2 hours. The low-boiling components were distilled off under reduced pressure. Then, water was added, and the mixture was aged under reflux for 4 hours for deprotection. The low-boiling components were then removed again under reduced pressure to obtain a comparative compound 2. The results of the analysis confirmed that the chemical structure of the comparative compound 2 is represented by the following chemical formula.

[0159] [Chemical formula 16]

[0160]

[0161] [Comparative Synthesis Example 3]

[0162] In a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 581.78 g of undecylenic acid trimethylsilyl ester and 0.087 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 168.23 g of methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature at 70-80°C.

[0163] [Chemical formula 17]

[0164]

[0165] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 3 hours. The low boiling point components were distilled off under reduced pressure. Then, 190 g of ion exchange water was added and the mixture was aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain comparative compound 3. The results of the analysis confirmed that it was comparative compound 3 shown in the following chemical structural formula.

[0166] [Chemical formula 18]

[0167]

[0168] [Comparative Synthesis Example 4]

[0169] In a flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 304.20 g of undecylenic acid trimethylsilyl ester and 0.092 g of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were added, and 304.20 g of methylhydrogenpolysiloxane represented by the following general formula was added dropwise while maintaining the temperature at 70-80°C.

[0170] [Chemical formula 19]

[0171]

[0172] After the addition was completed, the reaction was confirmed to be complete by hydrogen generation method after aging at 110°C for 3 hours. The low boiling point components were distilled off under reduced pressure. Then, 171.6 g of methanol was added and aged under reflux for 4 hours for deprotection. The low boiling point components were then removed again under reduced pressure to obtain comparative compound 4. The results of the analysis confirmed that it was comparative compound 4 shown in the following chemical structural formula.

[0173] [Chemical formula 20]

[0174]

[0175] [Preparation of aqueous dispersion: Examples 5 to 8, Comparative Examples 1 to 12]

[0176] The ingredients shown in Table 1 and Table 2 below were added to a mayonnaise bottle, and zirconium oxide beads (YTZ balls, )160g. After dispersion using a paint shaker and separation of the beads, aqueous dispersions of Examples 5 to 6 and Comparative Examples 1 to 5 were obtained. Each aqueous dispersion was evaluated by the following method, and the results are shown in Table 1. It should be noted that the viscosity of each aqueous dispersion was measured using an EMD viscometer (manufactured by Tokyo Keiki) just after preparation (initial), after standing at room temperature for 4 days, and after standing at room temperature for 4 months, and five levels were evaluated according to the following criteria at that time point. It should be noted that when the dispersion is unstable and phase separation occurs, it is evaluated as "separated".

[0177] [Appearance evaluation of aqueous dispersion]

[0178] The appearance of the aqueous dispersion was observed immediately after preparation.

[0179] ○: The dispersion state was good, and a dispersion having a low viscosity was obtained.

[0180] ×: The dispersion state is poor and becomes a paste.

[0181] [Evaluation of aqueous dispersion after standing for 4 months]

[0182] 1: It is not suitable as a cosmetic raw material.

[0183] 2: Not suitable as a cosmetic raw material.

[0184] 3: Can be used as cosmetic raw material.

[0185] 4: Useful as a cosmetic raw material.

[0186] 5: Very useful as a cosmetic raw material.

[0187] [Table 1]

[0188]

[0189] (Note 1) Trade name: Isostearic acid EX (produced by Advanced Alcohol Industries, Ltd.).

[0190] (Note 2) Trade name: STR-100A-LP (manufactured by Sakai Chemical Industry Co., Ltd.).

[0191] *High viscosity, cannot be measured.

[0192] [Table 2]

[0193]

[0194] (Note 1) Trade name: Isostearic acid EX (produced by Advanced Alcohol Industries, Ltd.).

[0195] (Note 3) Trade name: FINEX 30S-LPT (manufactured by Sakai Chemical Industry Co., Ltd.).

[0196] *High viscosity, cannot be measured.

[0197] As shown in Tables 1 and 2, by using the carboxylic acid co-modified polyorganosiloxane of the examples, not only hydrophobic titanium oxide but also hydrophobic zinc oxide microparticles can be obtained as a powder composition of low-viscosity aqueous slurry (aqueous dispersion) in which these powders are stably dispersed in an aqueous phase. These aqueous slurries are useful as cosmetic raw materials, etc., and it is expected that by using the carboxylic acid co-modified polyorganosiloxane of the examples, it is possible to easily design an external agent composition such as a sunscreen cosmetic in which these powders are stably dispersed in an aqueous phase.

[0198] On the other hand, for the carboxylic acid-modified silicone and higher fatty acids of the comparative examples, for hydrophobic titanium oxide, there is also a substance that obtains a powder composition of a low-viscosity aqueous slurry (aqueous dispersion) that is stable to a certain extent, but for the microparticles of hydrophobic zinc oxide, it is confirmed that the aqueous slurry (aqueous dispersion) is rapidly thickened or phase separated from just after preparation to four days. Therefore, for the known carboxylic acid-modified silicone and higher fatty acids of the comparative examples, sometimes sufficient dispersibility cannot be achieved for a part of the hydrophobic microparticles, and a stable aqueous slurry, sunscreen cosmetics, and other external-use agent compositions cannot be achieved, and the degree of freedom of formulation design is insufficient, and it is possible that the stability of the obtained cosmetic raw materials and the performance of the external-use agent compositions such as cosmetics are insufficient.

[0199] [Formulation design and formulation examples]

[0200] The carboxylic acid co-modified polyorganosiloxane of the present invention can be used by replacing part or all of the carboxylic acid-modified silicone in the formulation examples of the external preparation composition of the known carboxylic acid-modified silicone. Specifically, the carboxylic acid-modified silicones of the examples or formulation examples disclosed in Patent Document 1 (International Patent Publication No. WO2015 / 159773), Patent Document 2 (International Patent Publication No. WO2020 / 036065), International Patent Applications (PCT / JP19 / 029957, PCT / JP19 / 029927), International Patent Publication WO / 2020 / 036064, International Patent Publication WO / 2020 / 036061, International Patent Publication WO / 2020 / 036062, and International Patent Publication WO / 2020 / 036063 are replaced with the carboxylic acid co-modified polyorganosiloxane (Compounds 1 to 4) of Examples 1 to 4 as formulation examples of the cosmetics of the present invention and are included in the scope of the present invention, and the applicant of the present case clearly teaches such use and formulation design.

Claims

1. A carboxylic acid co-modified polyorganosiloxane represented by the following structural formula (1) which is liquid at 50°C. Structural formula (1): [Chemical formula 1] In the formula, R 1 is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms or a hydrogen atom, R 2 is a substituted or unsubstituted linear or branched monovalent hydrocarbon group having 6 to 30 carbon atoms, L 1 is one or more groups selected from the group represented by the following general formula (2), (2') and (2"), that is, a silylalkyl group having a siloxane dendron structure represented by the following general formula (2) when i=1: [Chemical formula 2] In the formula, R 1 is the same group as described above, R C is an alkyl group with 1 to 6 carbon atoms or a phenyl group, Z is a divalent organic group, and i represents L i The number of layers of the silylalkyl group shown in the figure is an integer of 1 to c when the number of layers as the number of repetitions of the silylalkyl group is c, and the number of layers c is an integer of 1 to 10, L i+1 When i is less than c, it is the silylalkyl group; when i=c, it is methyl or phenyl. i is 0; A chain-like organosiloxane group represented by the following general formula (2'): [Chemical formula 3] In the formula, R 11 are independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms, a hydroxyl group or a hydrogen atom, and R 11 At least one of them is the monovalent hydrocarbon group, t is a number in the range of 2 to 10, and r is a number in the range of 1 to 500; and The chain-like organosiloxane group represented by the following general formula (2"): [Chemical formula 4] In the formula, R 11 and r as above, Rc represents the general formula -Rc 1 -(ORc 2 )p-(O)w-Rc 3 -COOH-containing organic group, wherein Rc 1 represents a linear or branched alkylene group having 2 to 22 carbon atoms, Rc 2 represents a linear or branched alkylene group having 2 to 4 carbon atoms, Rc 3 represents a bond - or a linear or branched alkylene group having 1 to 22 carbon atoms, p represents a number from 0 to 200, and w represents a number of 0 or 1, R' is independently selected from the R 1 , R 2 , L 1 and the groups in Rc, n1+n2+n3+n4 is a number in the range of 1 to 1000, n1 is a number in the range of 0 to 999, n2 is a number in the range of 0 to 100, n3 is a number in the range of 1 to 100, n4 is a number in the range of 0 to 100, and when n4=0, at least one of R' is Rc.

2. The carboxylic acid co-modified polyorganosiloxane according to claim 1, wherein In formula (1), L 1 is a functional group represented by the following general formula (2-1), general formula (2-2) or general formula (2'), General formula (2-1): [Chemical formula 5] General formula (2-2): [Chemical formula 6] In the formula, R 1 , R C and Z is the same group as described above, a 1 and a 2 are each independently a number in the range of 0 to 3, General formula (2'): [Chemical formula 7] In the formula, R 11 They are each independently the same group as described above, t is a number in the range of 2 to 10, and r is a number in the range of 1 to 500.

3. The carboxylic acid co-modified polyorganosiloxane according to claim 1 or 2, characterized in that: In the structural formula (1), n1+n2+n3+n4 is a number in the range of 2 to 50, n1 is a number in the range of 0 to 49, n2 is a number in the range of 0 to 10, n3 is a number in the range of 1 to 10, n4 is a number in the range of 0 to 10, and when n4=0, at least one of R' is Rc.

4. The carboxylic acid co-modified polyorganosiloxane according to claim 1, characterized in that: It is liquid at room temperature, i.e., 25°C. In the structural formula (1), n1+n2+n3+n4 is a number in the range of 2 to 20, n3 is a number in the range of 1 to 10, n4 is a number in the range of 1 to 10, and (n1+n2+n3) / n4 is in the range of 0.1 to 5.

0.

5. A carboxylic acid co-modified polyorganosiloxane composition comprising: (A) the carboxylic acid co-modified polyorganosiloxane according to any one of claims 1 to 4; (B) a basic compound; and (C) at least one hydrophilic medium selected from the group consisting of water, polyols and lower alcohols.

6. A powder treatment agent comprising: The carboxylic acid co-modified polyorganosiloxane according to any one of claims 1 to 4 or the carboxylic acid co-modified polyorganosiloxane composition according to claim 5.

7. A surfactant or surface treatment agent comprising: The carboxylic acid co-modified polyorganosiloxane according to any one of claims 1 to 4 or the carboxylic acid co-modified polyorganosiloxane composition according to claim 5.

8. A powder composition comprising: (A) the carboxylic acid co-modified polyorganosiloxane according to any one of claims 1 to 4; (B) basic compounds; (C) one or more hydrophilic media selected from water, polyols and lower alcohols; and (D) Powder or colorant.

9. The powder composition according to claim 8, characterized in that The component (D) is (D1) a hydrophobic powder or a colorant, and the powder composition has a structure in which the component (D) is dispersed in an aqueous phase.

10. The powder composition according to claim 8, characterized in that The component (D) is (D1-1) hydrophobized titanium oxide microparticles or hydrophobized zinc oxide microparticles having an average particle size in the range of 1 to 200 nm, and the powder composition has a structure in which the component (D) is dispersed in an aqueous phase.

11. A composition for external use, comprising: The carboxylic acid co-modified polyorganosiloxane according to any one of claims 1 to 4 or the carboxylic acid co-modified polyorganosiloxane composition according to claim 5.

12. A composition for external use, comprising: (A) the carboxylic acid co-modified polyorganosiloxane according to any one of claims 1 to 4; (B) basic compounds; (C) one or more hydrophilic media selected from water, polyols and lower alcohols; and (D) powder or coloring agent, The external preparation composition has a structure in which the component (D) is dispersed in an aqueous phase.

13. An external-use composition comprising the powder composition according to any one of claims 8 to 10.

14. The composition for external use according to any one of claims 11 to 13, wherein The external-use composition is a cosmetic or a medicine.

15. A method for producing a composition for external use, which is the method for producing a composition for external use as described in any one of claims 12 to 14, comprising the following steps: (A) the carboxylic acid co-modified polysiloxane as described in any one of claims 1 to 4, (B) a basic compound, (C) one or more hydrophilic media selected from water, polyols and lower alcohols, and (D) a powder or a colorant are mixed in advance and formulated in the form of an aqueous dispersion of component (D).

Citation Information

Patent Citations

  • Powder for cosmetic and cosmetic containing the same

    JP1997059125A

  • Surface treatment agent, surface-treated powder and cosmetic preparation

    WO2009022621A1

  • Cosmetic

    WO2015159773A1

  • Oil-in-water emulsion cosmetic composition

    WO2020036061A1

  • Oil-in-water emulsion cosmetic

    WO2020036062A1