Co-modified organopolysiloxane and its use
By using linear, low-polymerization co-modified organopolysiloxane, the problems of thickening and reduced fluidity of powder treatment agents in the low HLB region in the existing technology are solved, and the processing of various oil agents is realized. The excellent affinity and compatibility form a stable powder dispersion, which is suitable for external preparation compositions such as cosmetics.
Patent Information
- Application Number
- CN202180062975.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-10-06
AI Technical Summary
Existing siloxanes for powder processing tend to thicken and reduce the fluidity of oil powder dispersions in the low HLB region, and have insufficient affinity for various oils, making it difficult to form stable powders over time. Dispersions.
A linear, low-polymerization co-modified organopolysiloxane is used, with an HLB range of 0.5 to 2.0 and a viscosity of 200 to 1500 mPa·s. It contains specific hydrophilic groups and long-chain hydrocarbon groups, and can interact with A variety of oil agents form excellent affinity and compatibility, and are used as powder treatment agents to form stable powder dispersions in oil.
It achieves high affinity and compatibility with various oils, avoids poor dispersion and thickening of powder, and forms a good and stable slurry over time, which is suitable for external use compositions such as cosmetics.
Smart Images

Figure CN116096787B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a co-modified organopolysiloxane and its use. The co-modified organopolysiloxane has a specific silicon-containing organic group, a hydrophilic group, and a specific hydrocarbon group such as a long-chain alkyl group at a specific ratio in the molecule, and has a certain HLB (Hydrophilic Lipophilic Balance) value and viscosity. Therefore, the co-modified organopolysiloxane has excellent affinity with a variety of oil agents and is highly useful as a powder treatment agent. Background Art
[0002] In external preparation compositions including cosmetics, various powders represented by white pigments such as titanium oxide and coloring pigments, body pigments such as mica, and powder dispersions thereof in oils are widely used as cosmetic raw materials, etc. In order to improve the dispersibility and blending stability of cosmetic raw materials and the touch / function of cosmetics containing powders, powders obtained by surface treatment of powders with various siloxane components are used (for example, Patent Documents 1 to 6). However, the performance of conventional siloxanes for powder treatment is insufficient. The applicant of this case proposed a co-modified organopolysiloxane copolymer and its application as a powder treatment agent, which is low molecular weight and low viscosity and has: a group having a carbosiloxy dendritic structure, a hydrophilic group such as a glycerol derivative, and an alkyl group in the molecule (Patent Document 7).
[0003] On the other hand, the co-modified organopolysiloxane specifically disclosed in Patent Document 7 achieves high powder dispersibility compared to conventional siloxane components, but when a powder dispersion is formed with an oil in a part of the low HLB region, thickening and reduction in fluidity may occur over time, and its stability over time leaves room for improvement. In addition, in recent years, from the perspective of further improving the degree of freedom in formula design of cosmetics, etc., the market has demanded a co-modified organopolysiloxane that has a high affinity for a wider range of oils and can form a powder dispersion with excellent stability over time.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 07-53326 (Japanese Patent No. 2719303)
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 10-167946
[0008] Patent Document 3: Japanese Patent Application Publication No. 2002-38013
[0009] Patent Document 4: International Patent Publication No. WO2011 / 049246
[0010] Patent Document 5: International Patent Publication No. WO2011 / 049248
[0011] Patent Document 6: International Patent Publication No. WO2011 / 136394
[0012] Patent Document 7: Japanese Patent Application Publication No. 2013-151657 (Japanese Patent Publication No. 6369887) Summary of the invention
[0013] Problems to be solved by the invention
[0014] The present invention is made to solve the above-mentioned technical problems, and its purpose is to provide a co-modified organopolysiloxane, which has excellent affinity and compatibility with a wide range of cosmetic raw materials (especially different types of oils), and when used in combination with powders, it is not easy to cause thickening and poor dispersion, and can form a good and stable slurry. In addition, the purpose of the present invention is to provide a powder treatment agent containing the organopolysiloxane, a powder surface-treated by the powder treatment agent, a powder composition containing the co-modified organopolysiloxane copolymer, and further provide an oil-in-oil powder dispersion containing an oil and an external agent composition containing these, in particular, to provide a cosmetic and its production method.
[0015] Solutions for solving problems
[0016] The present inventors have conducted intensive research and found that the above technical problems can be solved by using the following linear co-modified organopolysiloxane with a low degree of polymerization, thereby achieving the present invention. The co-modified organopolysiloxane has an HLB range of 0.5 to 2.0 and a viscosity range of 200 to 1500 mPa·s at 25°C, and has a specific hydrophilic group (Q); a C6 to 30 long-chain hydrocarbon group (R2); and an organic group (L1) containing silicone, which is selected from a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromonomer structure. In addition, it was found that the above technical problems can be solved by using a powder treatment agent and a powder composition containing the co-modified organopolysiloxane, and further using a powder dispersion in oil containing an oil agent and an external agent composition containing these, especially a cosmetic for cosmetics and a method for producing the same, thereby achieving the present invention. It should be noted that the co-modified organopolysiloxane of the present invention has excellent affinity and compatibility not only for silicone oil, but also for non-silicone organic oil agents (e.g., hydrocarbon oils and fatty acid ester oils), and can therefore be particularly preferably used in external preparation compositions such as cosmetics containing powders that use different types of oil agents in combination.
[0017] Beneficial Effects
[0018] According to the present invention, a co-modified organopolysiloxane can be provided, which has excellent affinity and compatibility with a wide range of cosmetic raw materials (especially different types of oils), and when used in combination with powders, it is not easy to cause thickening and poor dispersion, and can form a good and stable slurry. In addition, according to the present invention, a powder treatment agent containing the organopolysiloxane, a powder obtained by surface treatment using the powder treatment agent, and a powder composition containing the co-modified organopolysiloxane copolymer can be provided, and further a powder dispersion in oil containing an oil and an external agent composition containing these can be provided, especially a cosmetic for use and a method for producing the same. DETAILED DESCRIPTION
[0019] Hereinafter, the co-modified organopolysiloxane of the present invention, its application as various treatment agents (surfactants or surface treatment agents), in particular, its application as a powder treatment agent and its application as a raw material for cosmetics are described in detail. In addition, the powder dispersion in oil, the external preparation formed using the co-modified organopolysiloxane of the present invention, preferably the cosmetic, and particularly preferably the cosmetic for cosmetics are described in detail. It should be noted that the co-modified organopolysiloxane of the present invention can be used for the same purposes as the co-modified organopolysiloxanes described in the above-mentioned patent document 5 (International Publication Patent No. WO2011 / 049248) and patent document 7 (Japanese Patent Publication No. 2013-151657), and can be used to replace part or all of the co-modified organopolysiloxanes disclosed in these patent documents. Furthermore, regarding the dosage forms, types, and formulation examples of cosmetics and the like disclosed in these patent documents, cosmetics, powder dispersions, emulsions, and the like can be provided by replacing a part or all of the co-modified organopolysiloxane used therein with the co-modified organopolysiloxane of the present invention, and the present invention strongly suggests such formulation design.
[0020] The co-modified organopolysiloxane of the present invention is characterized in that the co-modified organopolysiloxane is a chain polysiloxane with a trimethylsiloxy terminal as represented by the structural formula (1) described later, and has at its side chain portion in a specific ratio: an organic group (L1) containing silicone, selected from a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromolecular monomer structure; a specific hydrophilic group (Q); and a long-chain hydrocarbon group (R2) having 6 to 30 carbon atoms, and the HLB of the co-modified organopolysiloxane is in the range of 0.5 to 2.0, and the viscosity at 25°C is in the range of 200 to 1500 mPa·s.
[0021] In the present invention, the hydrophilic-lipophilic balance (HLB) value refers to the value defined by "(total molecular weight of the hydrophilic group part / total molecular weight) × 20". For the co-modified organopolysiloxane of the present invention, this value needs to be in the range of 0.5 to 2.0. In particular, from the perspective of performance as a powder dispersant, it can be in the range of 1.1 to 2.0, and is particularly preferably in the range of 1.5 to 2.0. In the structural formula (1) described below, the values of a to d, especially the value of c that affects the number of bonds of the hydrophilic group (Q), need to be a value that satisfies the above range for the HLB value of the entire molecule.
[0022] When the HLB value is outside the above range, in particular, when the HLB value is less than the above lower limit, that is, when the content of the hydrophilic group (Q) in the molecule is small, even if it is the co-modified organopolysiloxane represented by the structural formula (1), it is not possible to fully cover the solid surface, and the slurry may tend to thicken over time, and the performance as a powder treatment agent may become insufficient. On the other hand, when the HLB value is greater than 2.0, that is, when the content of the hydrophilic group in the molecule increases, the hydrophilic group (Q) of the present invention is preferably an organic group containing a diglycerol derivative group, a sugar alcohol modified group, etc., which has a large number of hydroxyl groups, and therefore there is a tendency for the viscosity of the co-modified organopolysiloxane itself to increase due to the cohesive force generated by hydrogen bonds, and when used as a powder treatment agent, its handling workability may become insufficient.
[0023] As described above, the co-modified organopolysiloxane of the present invention needs to have a viscosity in the range of 200 to 1500 mPa·s at 25°C from the perspective of its operability as a powder treatment agent. In particular, from the perspective of affinity for non-silicone organic oil agents (e.g., hydrocarbon oils and fatty acid ester oils), the viscosity is preferably in the range of 300 to 1450 mPa·s, and more preferably in the range of 700 to 1450 mPa·s. Even if the co-modified organopolysiloxane has the above HLB and has a specific hydrophilic group, a silicone-containing organic group, and a monovalent hydrocarbon group having 6 to 30 carbon atoms, if its viscosity exceeds the above upper limit, the workability as a powder treatment agent is reduced. In particular, when a non-silicone-based organic oil agent (for example, hydrocarbon oil and fatty acid ester oil) is used to prepare a powder dispersion, the work efficiency and dispersibility become insufficient. In addition, the obtained powder dispersion (especially, a slurry as a powder dispersion in oil) thickens over time or the powder is insufficiently dispersed, making it difficult to use it as a cosmetic raw material. In addition, depending on the conditions, it is sometimes impossible to prepare a powder dispersion at all.
[0024] It should be noted that the viscosity of the co-modified organopolysiloxane is greatly affected by the type and content of the hydrophilic group (Q) and the polymerization degree n1 to n4 of each diorganosiloxy unit in the general formula (1) and their sum (n1+n2+n3+n4). Therefore, the values of n1 to n4 in the structural formula (1) need to be numbers that satisfy the above-mentioned viscosity range. It is particularly preferred that the range of (n1+n2+n3+n4) is 8 to 25, and it is particularly preferred that n1 is 3 to 10, n2 is 1 to 10, n3 is 0.1 to 10, and n4 is 0.5 to 2.0.
[0025] The co-modified organopolysiloxane of the present invention is represented by the following structural formula (1).
[0026] [Chemical formula 1]
[0027]
[0028] In the formula, R 1 A substituted or unsubstituted monovalent hydrocarbon group with 1 to 30 carbon atoms or a hydrogen atom, excluding other groups meeting the requirements of R 2 , L 1 The group represented by Q is preferably a methyl group or a phenyl group from an industrial point of view.
[0029] R 2 It is a substituted or unsubstituted linear or branched monovalent hydrocarbon group having 6 to 30 carbon atoms, and can improve the affinity with non-silicone oils such as hydrocarbon oils (cosmetic raw materials). 2 Examples of the alkyl group having 6 to 30 carbon atoms include hexyl, heptyl, octyl, decyl, dodecyl, undecyl, and hexadecyl groups, and an alkyl group having 8 to 20 carbon atoms is particularly preferred.
[0030] L 1 It is an organic group containing silicone selected from a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromer structure, and specifically, it is one or more groups selected from a silylalkyl group having a siloxane dendron structure described in the following general formula (2) when i=1, a chain organic siloxane group represented by the following general formula (2'), and a chain organic siloxane group represented by the following general formula (2")
[0031] [Chemical formula 2]
[0032]
[0033] (Where R 1 For the R 1 The same group, R C is an alkyl group having 1 to 6 carbon atoms or a phenyl group, and Z is a divalent organic group. i represents L i The layer number of the silylalkyl group is c, i is an integer from 1 to c, the layer number c is an integer from 1 to 10, and L i+1 When i is less than c, it is the silylalkyl group; when i=c, it is a methyl group or a phenyl group. i A number in the range of 0 to 3)
[0034] [Chemical formula 3]
[0035]
[0036] (Where R 11 are independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms, a hydroxyl group or a hydrogen atom, and R 11 At least one of them is the monovalent hydrocarbon group. t is a number in the range of 2 to 10, and r is a number in the range of 1 to 500)
[0037] [Chemical formula 4]
[0038]
[0039] (Where R 11 and r as above)
[0040] L 1 The groups shown are optionally the same or different. For example, in the same molecule, there may be: a silylalkyl group having a carbosiloxy dendron structure and a group having a siloxane macromer structure, the silylalkyl group may be a combination of organic groups containing silicone with different branching degrees (generations), and the group having a siloxane macromer structure may be a combination of organic groups containing silicone with different polymerization degrees.
[0041] L 1 The group shown may be a silylalkyl group having a carbosiloxane dendrimer structure, which is defined as a silylalkyl group represented by the above general formula (2) when i=1. The silylalkyl group having a carbosiloxane dendrimer structure has a structure in which the carbosiloxane unit is extended into a dendrimer shape, and is therefore a functional group having high water repellency compared to a linear or merely branched polysiloxane unit. Without impairing the touch derived from the hydrophilic functional group, the co-modified organopolysiloxane of the present application can provide an excellent surfactant and powder treatment agent. In addition, the silylalkyl group having a carbosiloxane dendrimer structure is chemically stable, and is therefore a functional group that imparts advantageous properties that can be used in combination with a wide range of cosmetic ingredients.
[0042] In the general formula (2), R C It is an alkyl group having 1 to 6 carbon atoms or a phenyl group, and industrially preferably a methyl group or a phenyl group.
[0043] In the general formula (2), i represents L 1 The layer number of the silylalkyl group is c, i is an integer from 1 to c, the layer number c is an integer from 1 to 10, and L i+1 When i is less than c, it is the silylalkyl group, and when i = c, it is a methyl group or a phenyl group. In particular, when i = c, it is preferably a methyl group.
[0044] The number of layers c is preferably an integer of 1 to 3 in industry, more preferably 1 or
[0045] 2. In each layer number, the group represented by L1 is as follows. In the formula, R2
[0046] and Z are the same groups as R2 and Z described above.
[0047] When the number of layers c=1, L1 is represented by the following general formula (2-1).
[0048] [Chemical formula 5]
[0049]
[0050] When the number of layers c=2, L1 is represented by the following general formula (2-2).
[0051] [Chemical formula 6]
[0052]
[0053] In formula (2), ai is independently a number in the range of 0 to 3, and in the structures represented by formulas (2-1) to (2-3) when the number of levels is 1 to 3, a1, a2, and a3 are independently a number in the range of 0 to 3. These ai are particularly preferably numbers in the range of 0 to 1, and ai is particularly preferably 0.
[0054] In the above formula, Z is independently a divalent organic group, specifically, a divalent organic group formed by addition reaction of a silicon-bonded hydrogen atom with a functional group having an unsaturated hydrocarbon group at the end, such as an alkenyl group, an acryloyloxy group, a methacryloyloxy group, etc., but it is not limited to these functional groups according to the method of introducing a silylalkyl group having a carbosiloxane dendron structure, and can be appropriately selected. Such functional groups are widely disclosed in Patent Document 7, etc., and Z in the present invention is preferably an alkylene group having 2 to 10 carbon atoms, and most preferably an ethylene group.
[0055] L 1 The group shown may be a group containing a siloxane macromolecular monomer structure bonded to the silicon atom constituting the main chain via oxygen or alkylene, which is hydrophobic and is a functional group showing a certain degree of water repellency / lipophilicity, and can provide the organopolysiloxane copolymer of the present application with an excellent surfactant and powder treatment agent without damaging the touch derived from the hydrophilic functional group. Specifically, L 1 The groups shown can be functional groups shown in the above general formula (2') and general formula (2"), where R 11 Industrially, methyl, phenyl or hydroxyl groups are particularly preferred, and R 11 One part is a methyl group and the other part is a long-chain alkyl group having 8 to 30 carbon atoms, R 11 At least one of them is a monovalent hydrocarbon group such as a methyl group, t is a number in the range of 2 to 10, and r is a number in the range of 1 to 500. From the viewpoint of compatibility with various oils, r is preferably a number in the range of 1 to 100, and particularly preferably a number in the range of 2 to 30.
[0056] Q is a hydrophilic group containing a sugar alcohol and represented by the following structural formulas (3-1) to (3-2) and bonded to a silicon atom via a divalent linking group (Z); and a hydrophilic group containing at least one hydrophilic unit selected from the hydrophilic units represented by the following structural formulas (3-3) to (3-5).
[0057] [Chemical formula 7]
[0058]
[0059] (wherein Z represents an alkylene group having 2 to 22 carbon atoms or -R 6 -C(=O)-OR 7 - the divalent organic group (R 6 is an alkylene group having 2 to 22 carbon atoms, R 7 is a group selected from ethylene, propylene, methylethylene or hexylene), m is 1 or 2)
[0060] [Chemical formula 8]
[0061]
[0062] (wherein Z is as described above, and m' is 0 or 1)
[0063] [Chemical formula 9]
[0064]
[0065] (W is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.)
[0066] [Chemical formula 10]
[0067]
[0068] [Chemical formula 11]
[0069]
[0070] The hydrophilic group Q is a portion that imparts hydrophilicity to the co-modified organopolysiloxane of the present application, and is generally a functional group derived from a hydrophilic compound. The molecular chain end of Q as defined above may be partially capped with a hydrocarbon, and preferably, examples thereof include functional groups derived from monovalent or higher alcohols, polyether compounds, (poly)glycerol compounds, (poly)glycidyl ether compounds, and hydrophilic sugars.
[0071] In the co-modified organopolysiloxane of the present invention, from the perspective of its properties as a powder treatment agent, especially from the perspective of the dispersion properties of inorganic powders, in the above structural formula (1), Q is preferably an organic group containing a polyol, and is particularly preferably a (poly)glycerol residue or a sugar alcohol residue. From the perspective of the performance as a powder treatment agent, especially from the perspective of suppressing the overall viscosity of the co-modified organopolysiloxane, Q is a hydrophilic group derived from a (poly)glycerol compound, and is most preferably a hydrophilic group derived from (poly)glycerol. Specifically, it is preferably a hydrophilic group derived from (poly)glycerol monoallyl ether, (poly)glyceryl eugenol, that is, a (poly)glycerol compound having a monoglycerol, diglycerol, triglycerol or tetraglycerol structure, and is most preferably a hydrophilic group as a diglycerol derivative.
[0072] The diglycerol derivative group is more preferably a diglycerol derivative group represented by the following structural formula (5).
[0073] -R 5 -OX m -H……(5)
[0074] In the formula, R 5 It is a divalent organic group that does not contain an oxyalkylene structure in which the average number of repetitions of the oxyalkylene unit is 2 or more, and is preferably an alkylene group having 2 to 10 carbon atoms. X is any hydrophilic unit selected from the hydrophilic units (=glycerol units) represented by the above structural formulas (3-3) to (3-5), and m is the number of repetitions of the glycerol unit, which is an average number in the range of 1.5 to 2.4. It should be noted that the average number of repetitions of each glycerol unit is in the range of 1.1 to 2.9, preferably the average number of repetitions is in the range of 1.5 to 2.4, more preferably in the range of 1.8 to 2.2, and most preferably an average of 2. That is, the glycerol derivative group as Q mainly contains a diglycerol derivative group. Here, the diglycerol derivative group preferably has a glycerol unit repetition structure without a branch, but may also have a structure in which a part of it has a branched structure such as a polyglyceryl group or a polyglycidyl ether group.
[0075] Most preferably, the diglycerol derivative group-containing organic group is an organic group containing a diglycerol derivative group represented by the following general formula (5-1) or the following general formula (5-2).
[0076] [Chemical formula 12]
[0077]
[0078] (Where R 5 represents a divalent organic group having no oxyalkylene structure in which the average number of repetitions of oxyalkylene units is 2 or more)
[0079] [Chemical formula 13]
[0080]
[0081] (Where R 5 As mentioned above)
[0082] In the co-modified organopolysiloxane of the present invention, the diglycerol derivative group-containing organic group is preferably a hydrophilic group derived from diglycerol monoallyl ether or diglyceryl eugenol. Most preferably, the diglycerol derivative group with m=2 in formula (5) is a pure product with a purity exceeding 98% by mass.
[0083] As for the organic group containing sugar alcohol as Q, the organic group containing sugar alcohol is particularly preferably the case where Z is a propylene group and m=1 in the structural formula (3-1). Similarly, the organic group containing sugar alcohol is particularly preferably the case where Z is a propylene group and m'=0 in the structural formula (3-2). The organic group containing sugar alcohol in this case corresponds to the structural formula (3-1) or (3-2), and is the structural formula: -C3H6-OCH2[CH(OH)]3CH2OH,
[0084] Or a xylitol residue represented by the structural formula: -C3H6-OCH{CH(OH)CH2OH}2.
[0085] In the structural formula (1), with respect to n1 to n4 representing the average degree of polymerization of each diorganosiloxy unit, (n1+n2+n3+n4) is a number in the range of 2 to 50, preferably a number in the range of 5 to 40, and particularly preferably a number in the range of 8 to 25. n1 is a number in the range of 0 to 20, and more preferably 3 to 10. n2 is a number in the range of 1 to 10, and more preferably 1.0 to 5.0. n3 is a number in the range of 0.1 to 10, and more preferably 0.1 to 5. n4 is a number in the range of 0.3 to 2.5, and more preferably 0.5 to 2.0. In addition, n4 affects the content of the hydrophilic group Q, and therefore it is particularly preferred that n4 is a number in the range of 0.5 to 2.0 for the HLB value of the entire molecule, and more preferably a number in the range of 1.5 to 2.0.
[0086] The co-modified organopolysiloxane of the present invention can be obtained by the following method: a compound having an organic group containing silicone (e.g., the silylalkyl group) having a carbon-carbon double bond at one end of the molecular chain, a hydrophilic compound having a reactive functional group such as an alkenyl group (e.g., diglyceryl allyl ether, etc.), and an unsaturated long-chain hydrocarbon compound having a carbon-carbon double bond at one end of the molecular chain are subjected to an addition reaction on an organopolysiloxane having a reactive functional group such as Si-H. The reaction preferably allows the raw materials to be subjected to an addition reaction on the organopolysiloxane having a reactive functional group such as Si-H in multiple stages. From the perspective of reaction control, purity, and yield, the addition reaction is preferably carried out in the presence of a hydrosilylation reaction catalyst. In addition, the crude co-modified organopolysiloxane obtained by the addition reaction can be purified by odorization treatment using a hydrogenation reaction in a solvent or without a solvent in the presence of a hydrogenation catalyst, or can be subjected to a low-odor treatment using an acidic substance. Furthermore, the co-modified organopolysiloxane of the present invention can also be obtained as a mixture with a hydrophilic compound having a reactive functional group such as an alkenyl group.
[0087] The synthesis of the co-modified organopolysiloxane of the present invention can be carried out by the same method as the reaction, purification, and odor reduction treatment using an acidic substance disclosed in paragraphs 0110 to 0122 of the above-mentioned Patent Document 5 (International Patent Publication No. WO2011 / 049248) by the applicant. In particular, from the perspective of being able to substantially deodorize the co-modified organopolysiloxane, it is preferred to treat with one or more acidic inorganic salts (preferably sodium hydrogen sulfate, etc.) characterized in that the acidic inorganic salt is solid at 25°C, is water-soluble, and has an aqueous solution having a pH of 4 or less at 25°C when 50 g of the salt is dissolved in 1 L of ion exchange water. For example, as described above, it refers to: (1) decomposition treatment, adding the above-mentioned acidic inorganic salt to the reaction system (for example, a reaction container such as a flask) of the co-modified organopolysiloxane composition synthesized by the hydrosilylation reaction, and stirring; (2) hydrolysis treatment, adding an acidic inorganic salt and water or an acidic inorganic salt, water and a hydrophilic solvent, and stirring; etc. The treatment step using the acidic inorganic salt is preferably carried out in the presence of water and / or a hydrophilic medium.
[0088] After the above-mentioned odor reduction treatment, it is preferable to include a stripping step of removing low boiling point fractions (such as propionaldehyde) as odor inducing substances. The above-mentioned treatment with an acidic substance and stripping of odor inducing substances are preferably performed multiple times.
[0089] Furthermore, from the viewpoint of reducing odor, it is preferred that after the acid treatment step, an alkaline buffer (sodium phosphate, potassium phosphate, sodium citrate, sodium acetate, sodium bicarbonate, etc.) in an amount equivalent to 100 ppm to 50,000 ppm is further added to the obtained co-modified organopolysiloxane or the composition containing the co-modified organopolysiloxane for neutralization.
[0090] From the viewpoint of removing unnecessary residues and the like from the co-modified organopolysiloxane of the present invention, filtration can be performed by a known method.
[0091] [Application of co-modified organopolysiloxane]
[0092] The novel co-modified organopolysiloxane of the present invention (hereinafter also referred to as "component (A)") is hydrophobic and has, in the same molecule, a silylalkyl group having a siloxane dendron structure that exhibits high water repellency and a hydrophilic group, and has low viscosity and generally low HLB, and is therefore excellent in operability, work efficiency, and stability in combination with lipophilic raw materials. It is therefore useful as a raw material component for various treatment agents and cosmetics, and is particularly useful as a surfactant or surface treatment agent for cosmetics, and particularly as a powder treatment agent or powder dispersant for surface treatment of powders and dispersion of powders.
[0093] The use of the novel co-modified organopolysiloxane of the present invention as a surfactant is common to the use of the co-modified organopolysiloxane as a surfactant and the preparation of each emulsion composition disclosed by the applicant in paragraphs 0124 to 0147 of the above-mentioned Patent Document 5 (International Patent Publication No. WO2011 / 049248). When preparing various emulsion compositions, the co-modified organopolysiloxane of the present invention (low viscosity, preferably low HLB) can also be used in combination with the co-modified organopolysiloxane disclosed in Patent Document 5 for emulsification.
[0094] [Application as powder treatment agent or powder dispersant]
[0095] The co-modified organopolysiloxane of the present invention has low viscosity and low HLB, and can be oriented on the surface of various powders to impart appropriate water resistance, and therefore can be preferably used as a powder surface treatment agent for the purpose of surface treatment and dispersion of cosmetic powders. In particular, the co-modified organopolysiloxane of the present invention is characterized in that, when used as a powder treatment agent, the dispersion stability in a mixed oil agent system, especially in a non-silicone organic oil agent, is further improved compared to known co-modified organopolysiloxanes, and further, after preparing a powder composition obtained by treating the surface of a powder with a treatment agent, even when a method of dispersing the powder composition in an oil agent as a dispersion medium is adopted, for powders that are difficult to be stably dispersed in conventional powder treatment agents, a powder dispersion in oil that is not easily aggregated, precipitated, or thickened over time and has excellent stability can be provided.
[0096] [Other uses]
[0097] The novel co-modified organopolysiloxane of the present invention can also be used as a touch improver, a moisturizer, an adhesive, or a skin adhesive. In addition, it can also be used as a film agent or a viscosity modifier by combining with water.
[0098] The co-modified organopolysiloxane of the present invention has good compatibility with various other hydrophilic and hydrophobic components in cosmetics, and can improve the dispersibility and stability of the powder in the cosmetics containing the powder. Therefore, the powder treatment agent of the present invention and the powder surface treatment agent of the present invention can improve the stability of the cosmetic containing the powder and the uniform dispersibility of the powder. Moreover, the cosmetic containing the powder surface-treated with the powder surface treatment agent is characterized in that the stability is high and the powder is uniformly dispersed in the cosmetic.
[0099] The amount of the co-modified organopolysiloxane in the powder treatment agent of the present invention is not particularly limited as long as the powder treatment effect can be exhibited, and can be, for example, 50 to 100% by weight, preferably 70 to 100% by weight, and more preferably 90 to 100% by weight.
[0100] When the co-modified organopolysiloxane of the present invention is used as a surface treatment agent for powder, the amount of the co-modified organopolysiloxane and the powder or colorant is preferably in the range of 0.1 to 30 parts by mass, particularly preferably 0.5 to 10 parts by mass, relative to 100 parts by mass of the powder or colorant. When the amount is less than the lower limit, the effect of the surface treatment may be insufficient, and when the treatment amount exceeds the upper limit, no further significant texture change occurs, and the tendency to form a uniform mixture of the powder and the co-modified organopolysiloxane increases.
[0101] The co-modified organopolysiloxane of the present invention can be used for treating the surface of a powder by a known method. The method is not particularly limited, and for example, the method can be appropriately selected from the following methods.
[0102] 1. A method of dispersing the target powder in a medium selected from an organic solvent containing a treatment agent to perform surface treatment.
[0103] 2. A method in which a powder is mixed with a powder treatment agent and then surface treated using a pulverizer such as a ball mill or a jet mill.
[0104] 3. A treatment method in which a treatment agent is mixed with a solvent, the powder is dispersed and adsorbed on the surface, and then dried to sinter.
[0105] 〔Powder composition〕
[0106] The present invention also relates to a powder composition comprising (A) the co-modified organopolysiloxane of the present invention and (B) a powder or a colorant. The powder composition can be obtained by mixing (B) a powder or a colorant with (A) the co-modified organopolysiloxane of the present invention by the above-mentioned method, etc., and the purpose is either surface treatment of the powder, improvement of the dispersibility of the powder, premixing for cosmetic raw materials, etc.
[0107] 〔Powder dispersion in oil〕
[0108] In addition, the powder dispersion in oil described in the present invention refers to a substance obtained by dispersing the powder composition obtained as described above in an oil agent, or a substance obtained by dissolving or dispersing the co-modified organopolysiloxane in an oil agent, adding the powder thereto, and mixing and dispersing, and its form is a liquid dispersion. This liquid dispersion is sometimes referred to as a "slurry". In particular, the co-modified organopolysiloxane of the present invention is useful in the following aspects: under the same conditions as the co-modified organopolysiloxane disclosed in the above-mentioned Patent Document 5, even an inorganic powder such as zinc oxide that cannot be fully processed can be prepared into a low-viscosity slurry.
[0109] The oil is not particularly limited as long as it can prepare a liquid dispersion. It is usually used as a component of a cosmetic and is usually liquid at room temperature, but may also be solid such as wax, or may be a high-viscosity and viscous gel or paste as described later. The oil is preferably (C) one or more oils selected from silicone oils, non-polar organic compounds, or low-polar organic compounds that are liquid at 5 to 100°C. It is particularly preferred to use (C1) silicone oils that are liquid at 5 to 100°C and (C2) one or more oils selected from hydrocarbon oils and fatty acid ester oils.
[0110] The dispersion in oil of the present invention can be appropriately prepared by a known method such as the following method.
[0111] 1. A method in which the powder composition obtained as described above is added to an oil such as ester oil or silicone oil and dispersed.
[0112] 2. A method in which the co-modified organopolysiloxane is dissolved or dispersed in the above-mentioned oil, powder is added thereto, and the mixture is mixed using a dispersing device such as a ball mill, a bead mill, or a sand mill.
[0113] Then, the obtained powder dispersion in oil can be blended directly into an external preparation composition (especially, a cosmetic).
[0114] The powder composition and dispersion in oil containing the co-modified organopolysiloxane of the present invention can be preferably used as an external preparation composition, and particularly preferably used as a cosmetic or a cosmetic raw material.
[0115] 〔(B) Powder or colorant〕
[0116] The (B) powder or colorant used in the powder composition and the powder dispersion in oil of the present invention is generally used as a component of cosmetics, including white and coloring pigments and extender pigments. White and coloring pigments are used for coloring cosmetics, etc., while extender pigments are used to improve the touch of cosmetics, etc. As the "powder" in the present invention, white and coloring pigments and extender pigments commonly used in cosmetics can be used without particular limitation. In the present invention, it is preferred to mix one or more powders. There is no limitation on the shape (spherical, rod-shaped, needle-shaped, plate-shaped, irregular, spindle-shaped, cocoon-shaped, etc.), particle size (smoke-shaped, microparticles, pigment grade, etc.) and particle structure (porous, non-porous, etc.) of the powder, and the average primary particle size is preferably in the range of 1nm to 100μm. In particular, when these powders or colorants are mixed as pigments, it is preferred to mix one or more selected from inorganic pigment powders, organic pigment powders, and resin powders with an average particle size in the range of 1nm to 20μm.
[0117] Examples of powders include inorganic powders, organic powders, surfactant metal salt powders (metal soaps), color pigments, pearlescent pigments, and metal powder pigments, and composites thereof may be used. In addition, surfaces thereof may be treated to be waterproof.
[0118] Their specific examples are the same as the powders or colorants disclosed in paragraphs 0150 to 0152 of the above-mentioned patent document 5 (International Publication No. WO2011 / 049248). As the powder used in the present invention, inorganic powders with ultraviolet absorption / scattering ability such as titanium oxide, zinc oxide, iron oxide, cerium oxide and their composites are preferred, and in particular, those obtained by waterproofing the surface are particularly preferred. The above-mentioned composite refers to a powder in which other inorganic particles are dispersed inside the surface-treated powder or inorganic powder.
[0119] The mixture of (A) the co-modified organopolysiloxane and (B) the powder or colorant is in the form of powder dispersed in the co-modified organopolysiloxane. The amount of the powder in the mixture is not particularly limited, but is preferably in the range of 50 to 99% by mass of the entire mixture, more preferably 80 to 90% by mass.
[0120] 〔(C) Oil〕
[0121] The oil used in the powder dispersion in oil of the present invention is preferably (C) one or more oils selected from silicone oil, non-polar organic compounds or low-polar organic compounds that are liquid at 5 to 100° C., and the non-polar organic compounds and low-polar organic compounds are preferably hydrocarbon oils and fatty acid ester oils.
[0122] In particular, the co-modified organopolysiloxane of the present invention has excellent affinity not only for the oil agent (C1) silicone oil that is liquid at 5 to 100°C, but also for the oil agent (C2) comprising one or more selected from hydrocarbon oil and fatty acid ester oil, and can form a stable powder dispersion in oil (slurry, etc.), so it is extremely useful as a mixed oil agent of the oil agent of component (C1) and the oil agent of component (C2); or a cosmetic raw material and external preparation composition containing them together.
[0123] In the oil, one or more selected from the well-known vegetable oils, animal oils, higher alcohols, liquid fatty acid triglycerides, artificial sebum, and fluorine oils can also be used. The co-modified organopolysiloxane also shows excellent dispersibility for these non-silicone oils, so hydrocarbon oils and fatty acid ester oils can be stably blended in cosmetics, and the moisturizing properties brought by these non-silicone oils can be maintained. Therefore, the co-modified organopolysiloxane can improve the temporal stability of these non-silicone oils in cosmetics.
[0124] In addition, by using hydrocarbon oil and / or fatty acid ester oil together with silicone oil, in addition to being able to impart a refreshing touch that is unique to silicone oil, it is also possible to retain moisture on the skin, impart a moisturizing feeling (also referred to as a "moist touch") and a smooth touch to the skin and hair of the cosmetic, and has the advantage of not damaging the stability of the cosmetic over time. Moreover, cosmetics containing hydrocarbon oil and / or fatty acid ester oil and silicone oil can apply these moisturizing ingredients (hydrocarbon oil and / or fatty acid ester oil) to the skin or hair in a more stable and uniform state, thereby improving the moisturizing effect of the moisturizing ingredients on the skin. Therefore, compared with cosmetics containing only non-silicone oil agents (hydrocarbon oils, fatty acid ester oils, etc.), cosmetics containing both non-silicone oil agents and silicone oils have the advantage of being able to impart a smoother and moist touch.
[0125] These oils are the same as those disclosed by the applicant in paragraphs 0130 to 0135 and paragraph 0206 of Patent Document 5 (International Patent Publication No. WO2011 / 049248). Examples of fluorine-based oils include perfluoropolyether, perfluorodecalin, and perfluorooctane.
[0126] The amount of the oil agent in the powder dispersion in oil of the present invention is not particularly limited, but is preferably in the range of 0.1 to 50% by mass, more preferably 0.5 to 25% by mass, in the cosmetic raw material.
[0127] The co-modified organopolysiloxane, the powder composition or the powder dispersion in oil containing the co-modified organopolysiloxane can be preferably used as an external application composition, especially a cosmetic or a cosmetic raw material. These external application compositions, especially external application compositions as cosmetics or medicines, are included in the invention of this application.
[0128] In particular, the co-modified organopolysiloxane, the powder composition or the powder dispersion in oil containing the co-modified organopolysiloxane are preferably used as raw materials for cosmetics, and the external preparation composition (including the form of cosmetics and medicines) containing them, especially various cosmetics, are included in the particularly preferred forms of the present invention.
[0129] The cosmetic of the present invention may further include: (D) water, alcohol such as ethanol (including use as a premix); (E) other surfactants; (F) polyols and / or lower monohydric alcohols; (G) inorganic salts and / or organic acid salts; (H) crosslinked organopolysiloxane, organopolysiloxane elastomer spherical powder, silicone resin, acrylic organosilicone dendrimer copolymer, organosilicone raw rubber, polyamide-modified organosilicone, alkyl-modified organosilicone wax, alkyl-modified organosilicone resin wax, organosilicone polyether elastomer gel, PITUITOUS SILICONE FLUIDS (viscous silicone fluids), liquid and slightly cross-linked organopolysiloxanes and other silicone components other than component (A); (J) water-soluble polymers; and (K) UV protection components (including inorganic and organic UV protection components / combination of UV protection components corresponding to UV-A and UV protection components corresponding to UV-B), which are common to the contents disclosed in paragraphs 0101 to 0113 of the above-mentioned patent document 7 (Japanese Patent Gazette No. 2013-151657).
[0130] In the cosmetic of the present invention, in addition to the above-mentioned components, various components such as oil-soluble gelling agents, organic modified clay minerals, antibacterial preservatives, physiologically active ingredients, skin beautifying ingredients, pH adjusters, antioxidants, solvents, chelating agents, moisturizing ingredients, fragrances, deodorants, etc. can be used within the scope that does not impair the purpose of the present invention. These optional components for cosmetics are the same as those disclosed in the above-mentioned patent document 7 (Japanese Patent Laid-Open No. 2013-151657) by the applicant, etc.
[0131] The topical composition of the present invention is not particularly limited as long as it is a composition applied to the human body as a cosmetic or a medicine. The cosmetic of the present invention, as a specific product, can be exemplified by: skin cosmetics such as skin cleansing products, skin care products, cosmetic products, antiperspirant products, and UV protection products; hair cosmetics such as hair cleansing products, hair styling products, hair coloring products, hair nourishing products, hair rinse products, hair conditioner products, and hair treatment products; and bath cosmetics. The medicine of the present invention can be exemplified by: hair growth agents, hair nourishing agents, analgesics, bactericides, anti-inflammatory agents, refreshing agents, and skin anti-aging agents, but are not limited thereto.
[0132] The type, form and container of the topical composition of the present invention are the same as those disclosed by the applicant in paragraphs 0230 to 0233 of the above-mentioned patent document 5 (International Patent Publication No. WO2011 / 049248), and the co-modified organopolysiloxane is particularly useful as a raw material for various cosmetics. The cosmetic of the present invention is most preferably a cosmetic containing the following substances: (A) the co-modified organopolysiloxane; (B) a powder or a colorant; (C1) a silicone oil that is liquid at 5 to 100°C; and (C2) an oil agent containing one or more selected from hydrocarbon oils and fatty acid ester oils.
[0133] Example
[0134] The present invention is specifically described below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. The viscosity (kinematic viscosity) is a value measured at 25°C. It should be noted that in the following composition formula, the Me3SiO group (or Me3Si group) is marked as "M", the Me2SiO group is marked as "D", and the MeHSiO group is marked as "D". H ", the unit formed by modifying the methyl group in D with an arbitrary substituent (R) is marked as D R .
[0135] (Example 1)
[0136] <Synthesis of Co-modified Organopolysiloxane Compound P1>
[0137] The reactor was charged with an average composition formula MD 5.2 D H 8.0 31.43 g of methyl hydrogen polysiloxane, 32.17 g of tris(trimethylsiloxy)vinylsilane, 27.11 g of hexadecene, and 9.28 g of diglycerol monoallyl ether shown in M were heated to 65°C while stirring under nitrogen flow. 0.02 g of platinum catalyst was added and the reaction was carried out for 10 hours. The reaction was confirmed to be completed by the alkaline decomposition gas generation method (using KOH ethanol / water solution to decompose the remaining Si-H groups and calculate the reaction rate based on the volume of hydrogen generated). Afterwards, the average composition formula MD was obtained by filtering. 5.2 D R1 3.2 D R2 1.3 D R3 3.5 M represents a diglycerol co-modified organopolysiloxane having a siloxane dendron structure.
[0138] In the formula, R 1 , R 2 and R 3The structure is shown below.
[0139] R 1 =-C2H4Si(OSiMe3)3.
[0140] R 2 =-C3H6O--X represents a hydrophilic group, wherein X is a diglycerol moiety.
[0141] R 3 =-C 16 H 33 .
[0142] The product is a light brown viscous translucent liquid.
[0143] (Example 2)
[0144] <Synthesis of Co-modified Organopolysiloxane Compound P2>
[0145] The reactor was charged with an average composition formula MD 5.2 D H 8.0 31.62 g of methyl hydrogen polysiloxane, 30.34 g of tris(trimethylsiloxy)vinylsilane, 27.27 g of hexadecene, and 10.77 g of diglycerol monoallyl ether were stirred and heated to 65°C under nitrogen flow. 0.02 g of platinum catalyst was added and the reaction was carried out for 10 hours. The reaction was confirmed to be completed by the alkaline decomposition gas generation method (using KOH ethanol / water solution to decompose the remaining Si-H groups and calculate the reaction rate based on the volume of hydrogen generated). Afterwards, the average composition formula MD was obtained by filtering. 5.2 D R1 3.0 D R2 1.5 D R3 3.5 M is a diglycerol co-modified organopolysiloxane having a siloxane dendron structure. In the formula, R 1 , R 2 and R 3 The same as Example 1. The product is a light yellow viscous transparent liquid.
[0146] (Example 3)
[0147] <Synthesis of Co-modified Organopolysiloxane Compound P3>
[0148] The reactor was charged with an average composition formula MD 18 D H 3.465.66g of methylhydrogenpolysiloxane, 2.27g of tris(trimethylsiloxy)vinylsilane, 25.72g of hexadecene, and 6.35g of diglycerol monoallyl ether shown in M were stirred and heated to 65°C under nitrogen flow. 0.02g of platinum catalyst was added and the reaction was carried out for 10 hours. The reaction was confirmed to be completed by the alkaline decomposition gas generation method (using KOH ethanol / water solution to decompose the remaining Si-H groups and calculate the reaction rate based on the volume of hydrogen generated). Afterwards, the average composition formula MD was obtained by filtering. 18 D R1 0.2 D R2 0.7 D R3 2.6 M is a diglycerol co-modified organopolysiloxane having a siloxane dendron structure. In the formula, R 1 , R 2 and R 3 The same as Example 1. The product is a light yellow viscous transparent liquid.
[0149] (Example 4)
[0150] <Synthesis of Co-modified Organopolysiloxane Compound P4>
[0151] The reactor was charged with an average composition formula MD 29 D H 7.3 57.78 g of methyl hydrogen polysiloxane, 11.25 g of tris(trimethylsiloxy)vinylsilane, 27.43 g of hexadecene, and 3.54 g of diglycerol monoallyl ether were stirred under nitrogen flow and heated to 65°C. 0.02 g of platinum catalyst was added and the reaction was carried out for 10 hours. The reaction was confirmed to be completed by the alkaline decomposition gas generation method (using KOH ethanol / water solution to decompose the remaining Si-H groups and calculate the reaction rate based on the volume of hydrogen generated). Afterwards, the average composition formula MD was obtained by filtering. 29 D R1 1.6 D R2 0.7 D R3 5.0 M is a diglycerol co-modified organopolysiloxane having a siloxane dendron structure. In the formula, R 1 , R 2 and R 3 The same as Example 1. The product is a light yellow viscous transparent liquid.
[0152] (Comparative Example 1)
[0153] <Synthesis of Co-modified Organopolysiloxane Compound R1>
[0154] The reactor was charged with an average composition formula MD 15 D H 3.0 M 61.26 g of methyl hydrogen polysiloxane, 32.32 g of tris(trimethylsiloxy)vinylsilane, and 6.42 g of diglycerol monoallyl ether were heated to 65°C while stirring under nitrogen flow. 0.02 g of platinum catalyst was added and the reaction was carried out for 10 hours. The reaction was confirmed to be completed by the alkaline decomposition gas generation method (using KOH ethanol / water solution to decompose the remaining Si-H groups and calculate the reaction rate based on the volume of hydrogen generated). Afterwards, the average composition formula MD was obtained by filtering. 16 D R1 2.4 D R2 0.6 M is a diglycerol co-modified organopolysiloxane having a siloxane dendron structure. In the formula, R 1 , R 2 The same as Example 1. The product is a light yellow viscous transparent liquid.
[0155] (Comparative Example 2)
[0156] <Synthesis of Co-modified Organopolysiloxane Compound R2>
[0157] The reactor was charged with an average composition formula MD 29 D H 7.3 58.53 g of methyl hydrogen polysiloxane, 7.30 g of tris(trimethylsiloxy)vinylsilane, 27.72 g of hexadecene, and 6.46 g of diglycerol monoallyl ether were stirred and heated to 65°C under nitrogen flow. 0.02 g of platinum catalyst was added and the reaction was carried out for 10 hours. The reaction was confirmed to be completed by the alkaline decomposition gas generation method (using KOH ethanol / water solution to decompose the remaining Si-H groups and calculate the reaction rate based on the volume of hydrogen generated). Afterwards, the average composition formula MD was obtained by filtering. 29 D R1 1.0 D R2 1.3 D R3 5.0 M is a diglycerol co-modified organopolysiloxane having a siloxane dendron structure. In the formula, R 1 , R 2 and R 3 The same as Example 1. The product is a light yellow viscous transparent liquid.
[0158] The average composition formula, HLB and viscosity of the co-modified organopolysiloxane compounds P1 to P4 obtained in Examples 1 to 4 and the comparative co-modified organopolysiloxane compounds R1 and R2 obtained in Comparative Examples 1 and 2 are summarized in Table 1. 1 , R 2 and R 3 The same as in Example 1.
[0159] [Table 1]
[0160]
[0161] [Evaluation of dispersion stability]
[0162] The above-mentioned co-modified organopolysiloxanes (recorded as P1 to R2 in the table) were dissolved or dispersed in an oil (ethylhexyl palmitate) according to the composition shown in Table 2, and powder (titanium oxide with an average particle size of 10×90 nm (product name STR-100A-LP, manufactured by Sakai Chemical Industry) and zirconium oxide beads (0.8 mmΦ) were added thereto, and mixed for 15 hours using a paint shaker (PAINT SHAKER, manufactured by Asada Iron Works Co., Ltd.) to prepare a powder dispersion (slurry). The results of evaluation based on the following evaluation criteria are shown in Table 2.
[0163] ○: Slurry viscosity is less than 2500 mPa·s.
[0164] Δ: The slurry viscosity is 2500 mPa·s or more.
[0165] ×: It is impossible to prepare a fluid slurry.
[0166] [Table 2]
[0167]
[0168] As shown in Table 1, in the co-modified organopolysiloxanes P1 to P4 of the present invention, ethylhexyl palmitate, which is a representative fatty acid ester oil, can form a low-viscosity slurry, but in the comparative compounds R1 and R2, no slurry can be prepared or a high-viscosity slurry can be obtained, and sufficient powder dispersion performance cannot be achieved in the fatty acid ester oil.
[0169] Regarding the co-modified organopolysiloxanes P1 to P3 of the present invention, slurries were prepared in the same manner except that 16 parts by mass of decamethylcyclopentasiloxane was used instead of 16 parts by mass of ethylhexyl palmitate, and the evaluation results are shown in Table 1. The evaluation criteria at this time are as follows.
[0170] ○○: The slurry viscosity is less than 1000 mPa·s, and there is no thickening over time.
[0171] 〇Δ: The slurry viscosity is less than 1000 mPa·s and thickens over time.
[0172] As shown in Table 2, the co-modified organopolysiloxane of the present invention, especially P1 and P2, can form a slurry with low viscosity and excellent temporal stability even for decamethylcyclopentasiloxane, and has excellent powder dispersibility for both silicone-based oils and non-silicone-based oils. It can be expected that the dispersion stability of powders can be improved in external preparation compositions and cosmetics obtained by using or using these oils in combination.
[0173] [Formulation Example]
[0174] In addition, regarding cosmetics using the co-modified organopolysiloxane of the present invention, [Formulation Example 1] W / O cushion foundation, [Formulation Example 2] W / O sunscreen, and [Other Formulation Examples] are disclosed in Japanese Patent Application No. 2020-160317.
Claims
1. A co-modified organopolysiloxane, wherein the co-modified organopolysiloxane is prepared according to HLB=(total molecular weight of the hydrophilic group part / total molecular weight)×20 The defined HLB value is in the range of 0.5 to 2.0, the co-modified organopolysiloxane is represented by the following structural formula (1), and has a viscosity at 25° C. in the range of 200 to 1500 mPa·s. Structural formula (1): In the formula, R 1 is a substituted or unsubstituted methyl group or a hydrogen atom; R 2 represents a substituted or unsubstituted linear or branched monovalent hydrocarbon group having 6 to 30 carbon atoms, L 1 is one or more groups selected from the group consisting of a silylalkyl group having a siloxane dendron structure represented by the following general formula (2) when i=1, a chain organosiloxane group represented by the following general formula (2'), and a chain organosiloxane group represented by the following general formula (2"), In the formula, R 1 is the same as R in the structural formula (1) 1 The same group, R C is an alkyl group or a phenyl group having 1 to 6 carbon atoms, Z is a divalent organic group; i represents L i The layer number of the silylalkyl group is c, i is an integer from 1 to c, the layer number c is an integer from 1 to 10, and L i+1 When i is less than c, it is the silylalkyl group; when i=c, it is a methyl group or a phenyl group; a i is a number in the range of 0 to 3, In the formula, R 11 are independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms, a hydroxyl group or a hydrogen atom, and R 11 At least one of them is the monovalent hydrocarbon group; t is a number in the range of 2 to 10, r is a number in the range of 1 to 500, In the formula, R 11 and r as above, Q is a hydrophilic group containing a sugar alcohol and represented by the following structural formulas (3-1) to (3-2) and bonded to a silicon atom via a divalent linking group (Z); and a hydrophilic group containing at least one hydrophilic unit selected from the hydrophilic units represented by the following structural formulas (3-3) to (3-5), In the formula, Z represents an alkylene group having 2 to 22 carbon atoms or -R 6 -C(=O)-OR 7 - a divalent organic group, wherein R 6 is an alkylene group having 2 to 22 carbon atoms, R 7 is a group selected from ethylene, propylene, methylethylene or hexylene, m is 1 or 2, Wherein, Z is as described above, m' is 0 or 1, In the formula, W is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, (n1+n2+n3+n4) is a number in the range of 2 to 50, n1 is a number in the range of 0 to 10, n2 is a number in the range of 1 to 10, n3 is a number in the range of 0.1 to 10, and n4 is a number in the range of 0.3 to 2.
5.
2. The co-modified organopolysiloxane according to claim 1, wherein In formula (1), L 1 is a functional group represented by the following general formula (2-1) or general formula (2-2), General formula (2-1): General formula (2-2): In the formula, R 1 , R C and Z is the same as R in formula (1), (2), (3-1) to (3-2) 1 , R C And the same group as Z, a 1 and a 2 Each independently represents a number in the range of 0 to 3.
3. The co-modified organopolysiloxane according to claim 1 or 2, wherein In the above formula (1), Q is a diglycerol derivative group-containing organic group bonded to a silicon atom via a divalent or higher linking group, and containing at least one glycerol unit selected from the glycerol units represented by the structural formulae (4-1) to (4-3) with an average number of repeating glycerol units in the range of 1.5 to 2.4, wherein the linking group excludes groups having an oxyalkylene structure with an average number of repeating oxyalkylene units of 2 or more, and the diglycerol derivative group-containing organic group excludes groups having an oxyalkylene structure with an average number of repeating oxyalkylene units of 2 or more.
4. The co-modified organopolysiloxane according to claim 1, characterized in that: In the above formula (1), Q is an organic group containing a diglycerol derivative group represented by the following general formula (5-1) or the following general formula (5-2), In the formula, R 5 represents a divalent organic group, except for a group having an oxyalkylene structure in which the average number of repetitions of oxyalkylene units is 2 or more, In the formula, R 5 As mentioned above.
5. The co-modified organopolysiloxane according to claim 1, wherein The HLB value is in the range of 1.5 to 2.
0. In formula (1), R 2 The co-modified organopolysiloxane has a viscosity at 25° C. in the range of 700 to 1450 mPa·s. 6 . A powder treatment agent, comprising the co-modified organopolysiloxane according to claim 1 .
7. A surfactant or a surface treatment agent, comprising the co-modified organopolysiloxane according to any one of claims 1 to 5.
8. A powder composition comprising: (A) the co-modified organopolysiloxane according to any one of claims 1 to 5 and (B) powder or colorant.
9. A powder dispersion in oil, comprising: (A) a co-modified organopolysiloxane as described in any one of claims 1 to 5; (B) a powder or a colorant; and (C) one or more oils selected from silicone oils, non-polar organic compounds or low-polar organic compounds that are liquid at 5 to 100°C. 10 . An external preparation composition comprising the co-modified organopolysiloxane according to claim 1 .
11. The external-use composition according to claim 10, wherein The topical composition contains: (A) the co-modified organopolysiloxane according to any one of claims 1 to 5; (B) a powder or a colorant; and (C) one or more oils selected from silicone oils, non-polar organic compounds or low-polar organic compounds that are liquid at 5 to 100°C.
Citation Information
Patent Citations
Catalytic reforming method
JP1988069887A
Make-up cosmetic
JP1995053326A
Composition good in dispensibility and skin-protecting agent containing the same
JP1998167946A
Powder composition, its powder-in-oil dispersion and cosmetic containing the same
JP2002038013A
Novel co-modified organopolysiloxane, and treatment agent and external use preparation comprising the same
JP2013151657A