A method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof
Through acid treatment, oxidation treatment and precise control of the pH of the alkalization end point, the separation and resource utilization of iron chromium and aluminum in the gasified slag activated acid solution are achieved, and the problems of complex processes and high energy consumption in the existing technology are solved. Efficient and economical resource utilization and environmental protection have been achieved.
Patent Information
- Application Number
- CN202111319448.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-11-09
AI Technical Summary
In the prior art, the gasification slag activated acid solution has complex treatment process, high energy consumption, and the treatment of high-salt wastewater cannot be effectively utilized, resulting in poor economic and environmental benefits.
The inert structure of the gasified slag is destroyed by acid treatment, and the active structure is formed, the oxidation treatment is carried out and the trivalent chromium is controlled not to be oxidized. Then, the co-precipitation of iron-chromium through precise control of the pH of the alkalization end point is induced to achieve the separation of iron-chromium and aluminum and its resources. Use.
It has achieved efficient detoxification and comprehensive utilization of gasified slag activated acid solution, and its products can be exported, with significant economic and environmental benefits, simple operation, low cost, zero emissions in the process, and is suitable for large-scale promotion.
Smart Images

Figure CN116102187B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic chemical industry, and relates to a method for detoxification of activated acid solution, and in particular to a method for detoxification of activated acid solution of gasified slag and comprehensive resource utilization thereof. Background Art
[0002] Coal gasification is the core technology for the clean utilization of coal resources. Under the background of carbon neutrality, coal gasification will be an important direction for the adjustment of the coal industry structure. With the large-scale promotion of coal gasification technology, more than 33 million tons of gasified slag are produced annually. Compared with raw coal, the heavy metal elements in gasified slag can be enriched 2-10 times. At present, acid activation process is mostly required for the treatment of gasified slag. CN108584971A discloses a method for preparing high modulus soluble silicate using gasified slag. The gasified slag needs to be pretreated with acid activation before controllable desiliconization. The heavy metals in the gasified slag will enter the activated acid solution during the acid activation process. The activated acid solution has a high acid concentration, complex composition, and is difficult to handle. How to safely and low-costly realize the detoxification and resource comprehensive utilization of the activated acid solution is an urgent problem to be solved.
[0003] CN111170509A discloses a method for treating a waste acid solution containing heavy metals, wherein the heavy metals in the waste acid solution are precipitated by synthesizing a sulfur-based precipitant. CN109626429A discloses a method for comprehensive treatment and utilization of chromium-containing waste acid, wherein the graded recovery and resource utilization of acid, iron and chromium are realized through gradual graded treatment. CN104310647A discloses a method for resource utilization of stainless steel pickling waste acid and wastewater treatment, wherein metal hydroxide is obtained by precipitation under alkaline conditions, and the product can be used as a raw material for stainless steel smelting. Although the above method can effectively remove heavy metals from acid solution, there are still problems such as complex process flow, multiple work sections, mixed products, high energy consumption, and inability to effectively utilize the high-salt wastewater after acid solution treatment.
[0004] It can be seen that how to develop a short-process, low-energy method for detoxification and comprehensive resource utilization of activated acid liquid to improve economic and environmental benefits has become an urgent problem that technical personnel in this field need to solve. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the present invention provides a method for detoxification of gasified slag activated acid solution and its comprehensive resource utilization. The method is simple to operate, low in cost, zero emission in the process, the product can be exported, the economic and environmental benefits are significant, and it is easy to promote and apply on a large scale.
[0006] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, characterized in that the method comprises the following steps:
[0008] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution;
[0009] (2) subjecting the gasified slag activated acid solution in step (1) to oxidation treatment to obtain a pre-oxidized activated acid solution;
[0010] (3) mixing the pre-oxidized activated acid solution of step (2) with an alkalizing agent, and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.2 to 2.8, to obtain an alkalized activated acid solution;
[0011] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0012] In the present invention, firstly, the inert Si-O-Al structure of the gasified slag is destroyed by acid treatment to form an active Si-OH structure, thereby obtaining an activated acid solution containing metal ions such as aluminum, iron, calcium, sodium, magnesium, and chromium; secondly, the activated acid solution is subjected to oxidation treatment to fully oxidize the divalent iron ions into trivalent iron ions, while controlling the trivalent chromium ions not to be oxidized, thereby achieving the purpose of reducing the precipitation pH of the trivalent chromium ions; then, an alkalizer is added to the pre-oxidized activated acid solution, and the pH of the alkalization endpoint is precisely controlled to induce the co-precipitation of iron and chromium, thereby achieving the simultaneous enrichment of iron and chromium; finally, by solid-liquid separation, an aluminum-calcium-rich detoxification activated acid solution and an iron-chromium precipitate are obtained, thereby achieving the separation and resource utilization of iron and chromium from aluminum.
[0013] In the present invention, the alkalinization endpoint pH in step (3) has a significant effect on the coprecipitation effect of ferric iron and trivalent chromium. When the alkalinization endpoint pH is less than 1.2, the coprecipitation rate of ferric iron and trivalent chromium is too low, resulting in poor detoxification effect of the activated acid solution; when the alkalinization endpoint pH is greater than 2.8, although the coprecipitation effect of ferric iron and trivalent chromium is good, trivalent aluminum will precipitate at this time, resulting in a loss of aluminum content in the aluminum-calcium detoxification activated acid solution, affecting its resource utilization.
[0014] As a preferred technical solution of the present invention, the gasified slag activation acid solution in step (1) comprises aluminum ions, iron ions, calcium ions, sodium ions, magnesium ions and chromium ions;
[0015] Preferably, according to the mass concentration, the gasified slag activation acid solution in step (1) comprises:
[0016]
[0017] Wherein, the mass concentration of Al can be 5g / L, 15g / L, 25g / L, 35g / L, 45g / L, 55g / L, 65g / L, 75g / L, 85g / L, 95g / L or 100g / L, etc., the mass concentration of Fe can be 5g / L, 15g / L, 25g / L, 35g / L, 45g / L, 55g / L, 65g / L, 75g / L, 85g / L, 95g / L or 100g / L, etc., the mass concentration of Ca can be 5g / L, 15g / L, 25g / L, 35g / L, 45g / L, 55g / L, 65g / L, 75g / L, 85g / L, 95g / L or 100g / L, etc., the mass concentration of Na can be 2g / L, 4g / L, 6g / L , 8g / L, 10g / L, 12g / L, 14g / L, 16g / L, 18g / L or 20g / L, etc. (excluding 0), the mass concentration of Mg can be 2g / L, 4g / L, 6g / L, 8g / L, 10g / L, 12g / L, 14g / L, 16g / L, 18g / L or 20g / L, etc. (excluding 0), the mass concentration of Cr can be 25ppm, 100ppm, 500ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, etc., but are not limited to the listed values, and other values not listed within the above numerical ranges are equally applicable.
[0018] Preferably, in step (1), H + The concentration is 0.5-10mol / L, such as 0.5mol / L, 1mol / L, 2mol / L, 3mol / L, 4mol / L, 5mol / L, 6mol / L, 7mol / L, 8mol / L, 9mol / L or 10mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] As a preferred technical solution of the present invention, the oxidant used in the oxidation treatment in step (2) includes any one of peroxide, hypochlorite or ozone, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of peroxide and hypochlorite, a combination of hypochlorite and ozone, a combination of ozone and peroxide, or a combination of peroxide, hypochlorite and ozone, etc.
[0020] Preferably, the amount of the oxidant is 1.0 to 1.5 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activation acid solution into trivalent iron ions, such as 1.1 times, 1.2 times, 1.3 times or 1.4 times, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0021] In the present invention, the amount of oxidant used in the oxidation treatment of step (2) has a significant effect on the oxidation rate of ferrous iron, thereby affecting the subsequent iron-chromium coprecipitation effect. When the amount of oxidant used is less than 1.0 times the theoretical amount of ferric iron generated by oxidizing ferrous iron, the oxidation rate of ferrous iron is too low, and the iron-chromium coprecipitation effect is poor; when the amount of oxidant used is greater than 1.5 times the theoretical amount of ferric iron generated by oxidizing ferrous iron, the amount of oxidant used is too much, and the iron-chromium coprecipitation effect is not significantly improved, resulting in a waste of oxidant.
[0022] As a preferred technical solution of the present invention, the temperature of the oxidation treatment in step (2) is 30-90°C, such as 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C or 85°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the oxidation treatment time in step (2) is 10 to 120 min, such as 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min or 110 min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the stirring rate of the oxidation treatment in step (2) is 50 to 350 rpm, such as 100 rpm, 150 rpm, 200 rpm, 250 rpm or 300 rpm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] As a preferred technical solution of the present invention, the alkalizing agent in step (3) includes any one of sodium hydroxide, calcium hydroxide, calcium oxide or calcium-based solid waste, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of sodium hydroxide and calcium hydroxide, a combination of calcium hydroxide and calcium oxide, a combination of calcium-based solid waste and sodium hydroxide, or a combination of sodium hydroxide, calcium hydroxide and calcium oxide.
[0026] As a preferred technical solution of the present invention, the temperature of the alkalization treatment in step (3) is 50-95°C, such as 55°C, 60°C, 65°C, 70°C, 75°C, 80°C or 85°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the time of the alkalization treatment in step (3) is 10 to 180 min, such as 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min or 170 min, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the stirring rate of the alkalization treatment in step (3) is 50 to 500 rpm, such as 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm or 450 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] In the present invention, the solid-liquid separation in step (4) includes any one of filtration, centrifugation or gravity sedimentation, or a combination of at least two of them.
[0030] In the present invention, the iron-chromium precipitate obtained in step (4) is subsequently washed and dried.
[0031] As a preferred technical solution of the present invention, the above-mentioned method for detoxification of gasified slag activated acid solution and its resource comprehensive utilization comprises the following steps:
[0032] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al 5-100 g / L, Fe 5-100 g / L, Ca 5-100 g / L, Na 0-20 g / L, Mg 0-20 g / L, Cr>20 ppm, H + The concentration is 0.5~10mol / L;
[0033] (2) using an oxidant to oxidize the gasified slag activated acid solution in step (1), wherein the amount of the oxidant is 1.0 to 1.5 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 30 to 90° C., the time is 10 to 120 min, and the stirring rate is 50 to 350 rpm to obtain a pre-oxidized activated acid solution;
[0034] (3) mixing the pre-oxidized activated acid solution of step (2) with an alkalizing agent and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.2 to 2.8, the temperature is 50 to 95° C., the time is 10 to 180 min, and the stirring rate is 50 to 500 rpm to obtain an alkalized activated acid solution;
[0035] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0036] The second object of the present invention is to provide an aluminum-calcium-rich detoxification activation acid solution and iron-chromium precipitate prepared by the method described in the first object.
[0037] The third object of the present invention is to provide an application of the aluminum-calcium-rich detoxification activation acid solution provided by the second object, and the aluminum-calcium-rich detoxification activation acid solution is used in the preparation of aluminum-based water purifiers and aluminum-calcium-based products.
[0038] The fourth object of the present invention is to provide an application of the ferro-chromium precipitate provided in the third object, wherein the ferro-chromium precipitate is used for preparing smelting raw materials and ferro-chromium alloys.
[0039] Compared with the prior art, the present invention has at least the following beneficial effects:
[0040] (1) The method provided by the present invention controls the reaction conditions. First, the inert Si-O-Al structure of the gasified slag is destroyed by acid treatment to form an active Si-OH structure, thereby obtaining an activated acid solution containing metal ions such as aluminum, iron, calcium, sodium, magnesium, and chromium. Second, the activated acid solution is subjected to an oxidation treatment to fully oxidize the divalent iron ions into trivalent iron ions, while controlling the trivalent chromium ions not to be oxidized, thereby achieving the purpose of lowering the precipitation pH of the trivalent chromium ions. Next, an alkalizing agent is added to the pre-oxidized activated acid solution, and the pH at the alkalization endpoint is precisely controlled to induce the co-precipitation of iron and chromium, while aluminum does not precipitate, thereby achieving the simultaneous enrichment of iron and chromium. Finally, the separation and resource utilization of iron and chromium and aluminum are achieved through solid-liquid separation. Under the optimal conditions, the iron precipitation rate can reach 84%, the chromium precipitation rate can reach 71%, and the aluminum precipitation rate can reach 0%.
[0041] (2) The aluminum-calcium-rich detoxification activation acid prepared by the present invention has a high aluminum content and a low heavy metal content, and can be used to prepare aluminum-based water purifiers (polyaluminum chloride, polyaluminum chloride iron) and aluminum-calcium-based products (calcium aluminate); the iron grade in the iron-chromium sludge is high, and can be used as a smelting raw material and iron-chromium alloy. The present invention simply and efficiently realizes the efficient detoxification and resource comprehensive utilization of gasification slag activation acid, has a simple operation process, reaction conditions at room temperature, low cost, zero emission in the process, and the product can be exported, with significant economic and environmental benefits, and is easy to promote and apply on a large scale.
[0042] (3) The method provided by the present invention can be extended to the treatment of acidic waste liquid containing iron, chromium and aluminum. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 A schematic flow chart of a method for detoxification of gasified slag activated acid solution and its comprehensive resource utilization provided in the specific implementation mode of the present invention.
[0044] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0045] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0046] Example 1
[0047] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0048] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Cr: 83 ppm, H + The concentration is 2.0 mol / L;
[0049] (2) using hydrogen peroxide to oxidize the gasified slag activated acid solution in step (1), wherein the amount of hydrogen peroxide used is 1.2 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 80° C., the time is 60 min, and the stirring rate is 300 rpm, to obtain a pre-oxidized activated acid solution;
[0050] (3) mixing the pre-oxidized activated acid solution of step (2) with sodium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 2.6, the temperature is 80° C., the time is 60 min, and the stirring rate is 300 rpm, to obtain an alkalized activated acid solution;
[0051] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0052] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 84.79%, the chromium precipitation rate is 71.21%, and the aluminum precipitation rate is 0.00%.
[0053] Example 2
[0054] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0055] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Cr: 83 ppm, H + The concentration is 4.0 mol / L;
[0056] (2) using hydrogen peroxide to oxidize the gasified slag activated acid solution in step (1), wherein the amount of hydrogen peroxide used is 1.2 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 40° C., the time is 60 min, and the stirring rate is 200 rpm, to obtain a pre-oxidized activated acid solution;
[0057] (3) mixing the pre-oxidation activated acid solution of step (2) with sodium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 2.2, the temperature is 60° C., the time is 60 min, and the stirring rate is 400 rpm, to obtain an alkalized activated acid solution;
[0058] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0059] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 80.26%, the chromium precipitation rate is 68.32%, and the aluminum precipitation rate is 0.00%.
[0060] Example 3
[0061] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0062] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Cr: 83 ppm, H + The concentration is 8.0 mol / L;
[0063] (2) using hydrogen peroxide to oxidize the gasified slag activated acid solution in step (1), wherein the amount of hydrogen peroxide used is 1.4 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 40° C., the time is 90 min, and the stirring rate is 200 rpm, to obtain a pre-oxidized activated acid solution;
[0064] (3) mixing the pre-oxidized activated acid solution of step (2) with sodium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.6, the temperature is 90° C., the time is 90 min, and the stirring rate is 350 rpm to obtain an alkalized activated acid solution;
[0065] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0066] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 74.25%, the chromium precipitation rate is 61.62%, and the aluminum precipitation rate is 0.00%.
[0067] Example 4
[0068] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0069] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Cr: 83 ppm, H + The concentration is 8.0 mol / L;
[0070] (2) using hydrogen peroxide to oxidize the gasified slag activated acid solution in step (1), wherein the amount of hydrogen peroxide used is 1.4 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 90° C., the time is 120 min, and the stirring rate is 350 rpm, to obtain a pre-oxidized activated acid solution;
[0071] (3) mixing the pre-oxidized activated acid solution of step (2) with sodium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.3, the temperature is 90° C., the time is 120 min, and the stirring rate is 350 rpm, to obtain an alkalized activated acid solution;
[0072] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0073] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 66.82%, the chromium precipitation rate is 58.75%, and the aluminum precipitation rate is 0.00%.
[0074] Example 5
[0075] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0076] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Cr: 83 ppm, H + The concentration is 8.0 mol / L;
[0077] (2) using hydrogen peroxide to oxidize the gasified slag activated acid solution in step (1), wherein the amount of hydrogen peroxide used is 1.0 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 30° C., the time is 120 min, and the stirring rate is 150 rpm, to obtain a pre-oxidized activated acid solution;
[0078] (3) mixing the pre-oxidized activated acid solution of step (2) with calcium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.8, the temperature is 95° C., the time is 150 min, and the stirring rate is 350 rpm to obtain an alkalized activated acid solution;
[0079] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0080] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 78.12%, the chromium precipitation rate is 65.66%, and the aluminum precipitation rate is 0.00%.
[0081] Example 6
[0082] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0083] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Cr: 83 ppm, H + The concentration is 8.0 mol / L;
[0084] (2) using sodium hypochlorite to oxidize the gasified slag activated acid solution in step (1), wherein the amount of sodium hypochlorite used is 1.5 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 90° C., the time is 20 min, and the stirring rate is 300 rpm, to obtain a pre-oxidized activated acid solution;
[0085] (3) mixing the pre-oxidized activated acid solution of step (2) with sodium hydroxide for alkalization treatment, wherein the end point pH of the alkalization treatment is 2.8, the temperature is 50° C., the time is 100 min, and the stirring rate is 350 rpm to obtain an alkalized activated acid solution;
[0086] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0087] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 82.12%, the chromium precipitation rate is 69.95%, and the aluminum precipitation rate is 0.00%.
[0088] Example 7
[0089] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0090] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 13.02 g / L, Fe: 16.71 g / L, Ca: 17.32 g / L, Na: 2.03 g / L, Mg: 1.45 g / L, Si: 0.08 g / L, Cr: 83 ppm, H + The concentration is 1.0 mol / L;
[0091] (2) using sodium hypochlorite to oxidize the gasified slag activated acid solution in step (1), wherein the amount of sodium hypochlorite used is 1.0 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 90° C., the time is 20 min, and the stirring rate is 300 rpm, to obtain a pre-oxidized activated acid solution;
[0092] (3) mixing the pre-oxidation activated acid solution of step (2) with carbide slag (a calcium-based solid waste: the main component is calcium hydroxide) and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.4, the temperature is 85° C., the time is 180 min, and the stirring rate is 400 rpm, to obtain an alkalized activated acid solution;
[0093] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0094] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 70.24%, the chromium precipitation rate is 58.86%, and the aluminum precipitation rate is 0.00%.
[0095] Example 8
[0096] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0097] Example 8
[0098] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0099] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 73.97 g / L, Fe: 68.24 g / L, Ca: 78.65 g / L, Na: 10.15 g / L, Mg: 13.22 g / L, Cr: 2950 ppm, H + The concentration is 4 mol / L;
[0100] (2) using hydrogen peroxide to oxidize the gasified slag activated acid solution in step (1), wherein the amount of hydrogen peroxide used is 1.2 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 80° C., the time is 90 min, and the stirring rate is 300 rpm, to obtain a pre-oxidized activated acid solution;
[0101] (3) mixing the pre-oxidized activated acid solution of step (2) with sodium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 2.6, the temperature is 80° C., the time is 120 min, and the stirring rate is 350 rpm, to obtain an alkalized activated acid solution;
[0102] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0103] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 82.73%, the chromium precipitation rate is 70.12%, and the aluminum precipitation rate is 0.00%.
[0104] Example 9
[0105] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0106] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 73.97 g / L, Fe: 68.24 g / L, Ca: 78.65 g / L, Na: 10.15 g / L, Mg: 13.22 g / L, Cr: 2950 ppm, H + The concentration is 6.0 mol / L;
[0107] (2) using ozone to oxidize the gasified slag activated acid solution in step (1), wherein the amount of ozone used is 1.2 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 70° C., the time is 30 min, and the stirring rate is 100 rpm, to obtain a pre-oxidized activated acid solution;
[0108] (3) mixing the pre-oxidized activated acid solution of step (2) with sodium hydroxide and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 2.0, the temperature is 80° C., the time is 60 min, and the stirring rate is 350 rpm, to obtain an alkalized activated acid solution;
[0109] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0110] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 79.82%, the chromium precipitation rate is 67.75%, and the aluminum precipitation rate is 0.00%.
[0111] Example 10
[0112] This embodiment provides a method for detoxification of gasified slag activated acid solution and comprehensive resource utilization thereof, and the process is as follows: Figure 1 As shown, the method comprises the following steps:
[0113] (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al: 73.97 g / L, Fe: 68.24 g / L, Ca: 78.65 g / L, Na: 10.15 g / L, Mg: 13.22 g / L, Cr: 2950 ppm, H + The concentration is 6.0 mol / L;
[0114] (2) using ozone to oxidize the gasified slag activated acid solution in step (1), wherein the amount of ozone used is 1.5 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 30° C., the time is 30 min, and the stirring rate is 100 rpm, to obtain a pre-oxidized activated acid solution;
[0115] (3) mixing the pre-oxidized activated acid solution of step (2) with an alkalizing agent and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.2, the temperature is 80° C., the time is 120 min, and the stirring rate is 350 rpm to obtain an alkalized activated acid solution;
[0116] (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
[0117] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 66.74%, the chromium precipitation rate is 56.12%, and the aluminum precipitation rate is 0.00%.
[0118] Embodiment 11
[0119] The present embodiment provides a method for detoxification of gasified slag by activated acid solution and its comprehensive resource utilization. Except for reducing the amount of oxidant in step (2) to 0.5 times the theoretical amount of ferric iron produced by oxidizing divalent iron, the other conditions are the same as those in Example 1 and are not described in detail here.
[0120] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 44.12%, the chromium precipitation rate is 32.65%, and the aluminum precipitation rate is 0.00%.
[0121] Compared with Example 1, the amount of oxidant used in this embodiment is reduced to less than 1.0 times the theoretical amount of ferric iron generated by oxidizing divalent iron, resulting in an excessively low oxidation rate of divalent iron in the activated acid solution, poor iron-chromium coprecipitation effect, and inability to achieve efficient detoxification.
[0122] Example 12
[0123] The present embodiment provides a method for detoxification of gasified slag by activated acid solution and its comprehensive resource utilization. In the method, except that the amount of oxidant in step (2) is increased to 2.0 times the theoretical amount of ferric iron produced by oxidizing divalent iron, the other conditions are the same as those in Example 1 and are not described in detail here.
[0124] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 85.31%, the chromium precipitation rate is 72.06%, and the aluminum precipitation rate is 0.00%.
[0125] Compared with Example 1, the amount of oxidant used in this embodiment is increased to 1.5 times greater than the theoretical amount of ferric iron generated by oxidizing divalent iron. The amount of oxidant used is too much, and the divalent iron in the activated acid solution has been completely oxidized to ferric iron. At this time, the main factor affecting the detoxification effect is the alkalinization endpoint pH, so the iron-chromium co-precipitation effect is not significantly improved, which will lead to a waste of oxidant.
[0126] Comparative Example 1
[0127] This comparative example provides a method for detoxification of gasification slag activated acid solution and its comprehensive resource utilization. Except for removing the oxidation treatment of the gasification slag activated acid solution in step (2), that is, directly alkalizing the gasification slag activated acid solution, the other conditions of the method are the same as those in Example 1, so they are not repeated here.
[0128] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 5.35%, the chromium precipitation rate is 1.52%, and the aluminum precipitation rate is 0.00%.
[0129] Compared with Example 1, this embodiment eliminates the oxidation treatment of the gasification slag activation acid solution. At this time, the iron in the activation acid solution mostly exists in the form of divalent ions and cannot be precipitated at low pH values. Therefore, during the alkalinization treatment process, it is impossible to induce co-precipitation of iron and chromium, and efficient detoxification of the activation acid solution cannot be achieved.
[0130] Comparative Example 2
[0131] This comparative example provides a method for detoxification of gasified slag activated acid solution and its comprehensive resource utilization. Except for reducing the pH value of the alkalization endpoint in step (3) to 0.8, the other conditions are the same as those in Example 1, so they are not described here.
[0132] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 15.44%, the chromium precipitation rate is 21.58%, and the aluminum precipitation rate is 0.00%.
[0133] Compared with Example 1, the alkalization endpoint pH in this comparative example is reduced to less than 1.2. At this time, the coprecipitation rate of trivalent iron and trivalent chromium is too low, resulting in poor detoxification effect of the activated acid solution.
[0134] Comparative Example 3
[0135] This comparative example provides a method for detoxification of gasified slag activated acid solution and its comprehensive resource utilization. Except for increasing the pH value of the alkalization endpoint in step (3) to 3.2, the other conditions are the same as those in Example 1, so they are not described here.
[0136] According to ICP-OES detection and calculation, in this embodiment, the iron precipitation rate is 95.04%, the chromium precipitation rate is 88.96%, and the aluminum precipitation rate is 62.29%.
[0137] Compared with Example 1, the alkalization endpoint pH in this comparative example is increased to greater than 2.8. Although the co-precipitation effect of trivalent iron and trivalent chromium is good at this time, the trivalent aluminum in the activated acid solution will precipitate, resulting in excessive loss of aluminum content in the aluminum-calcium-rich detoxification activated acid solution, affecting its resource utilization.
[0138] It can be seen that the method provided by the present invention induces co-precipitation of iron and chromium by pre-oxidation-precisely controlling pH alkalization, realizes the simultaneous enrichment of iron and chromium, and simply and efficiently realizes the separation of iron and chromium from aluminum in the gasification slag activation acid and the comprehensive resource utilization, the operation process is simple, the reaction conditions are room temperature, the cost is low, and the process has zero emissions; at the same time, the aluminum-calcium-rich detoxification activation acid prepared by the present invention has a high aluminum content and a low heavy metal content, and can be used to prepare aluminum-based water purifiers (polyaluminum chloride, polyaluminum chloride iron) and aluminum-calcium-based products (calcium aluminate); the iron grade in the iron-chromium precipitate is high, and can be used as a smelting raw material and iron-chromium alloy, and the product can be exported, with significant economic and environmental benefits; in addition, the method provided by the present invention can also be expanded to the treatment of acidic waste liquid containing iron, chromium, and aluminum, is easy to promote on a large scale, and has broad application prospects.
[0139] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0140] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0141] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0142] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for detoxification of gasified slag activated acid solution and its comprehensive resource utilization, characterized in that: The method comprises the following steps: (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution; the gasified slag activation acid solution comprises aluminum ions, iron ions, calcium ions, sodium ions, magnesium ions and chromium ions; (2) subjecting the gasified slag activated acid solution of step (1) to oxidation treatment to obtain a pre-oxidized activated acid solution; the amount of the oxidant used in the oxidation treatment is 1.0 to 1.5 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions; (3) mixing the pre-oxidized activated acid solution of step (2) with an alkalizing agent, and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.2 to 2.8, to obtain an alkalized activated acid solution; (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
2. The method according to claim 1, characterized in that According to the mass concentration, the gasified slag activation acid solution in step (1) comprises:
3. The method according to claim 1, characterized in that In step (1), the H in the gasified slag activation acid solution + The concentration is 0.5~10mol / L.
4. The method according to claim 1, characterized in that: The oxidant used in the oxidation treatment in step (2) includes one or a combination of at least two of peroxide, hypochlorite or ozone.
5. The method according to claim 1, characterized in that The temperature of the oxidation treatment in step (2) is 30 to 90°C.
6. The method according to claim 1, characterized in that The oxidation treatment time in step (2) is 10 to 120 minutes.
7. The method according to claim 1, characterized in that The stirring rate of the oxidation treatment in step (2) is 50 to 350 rpm.
8. The method according to claim 1, characterized in that The alkalizing agent in step (3) includes one or a combination of at least two of sodium hydroxide, calcium hydroxide, calcium oxide or calcium-based solid waste.
9. The method according to claim 1, characterized in that: The temperature of the alkalization treatment in step (3) is 50-95°C.
10. The method according to claim 1, characterized in that The alkalization treatment time in step (3) is 10 to 180 minutes.
11. The method according to claim 1, characterized in that: The stirring rate of the alkalization treatment in step (3) is 50 to 500 rpm.
12. The method according to claim 1, characterized in that The method comprises the following steps: (1) treating the gasified slag with acid to obtain a gasified slag activation acid solution, wherein the gasified slag activation acid solution comprises Al 5-100 g / L, Fe 5-100 g / L, Ca 5-100 g / L, Na 0-20 g / L, Mg 0-20 g / L, Cr>20 ppm, H + The concentration is 0.5~10mol / L; (2) using an oxidant to oxidize the gasified slag activated acid solution in step (1), wherein the amount of the oxidant is 1.0 to 1.5 times the theoretical amount required to oxidize all the divalent iron ions in the gasified slag activated acid solution into trivalent iron ions, the oxidation treatment temperature is 30 to 90° C., the time is 10 to 120 min, and the stirring rate is 50 to 350 rpm to obtain a pre-oxidized activated acid solution; (3) mixing the pre-oxidized activated acid solution of step (2) with an alkalizing agent and performing an alkalization treatment, wherein the end point pH of the alkalization treatment is 1.2 to 2.8, the temperature is 50 to 95° C., the time is 10 to 180 min, and the stirring rate is 50 to 500 rpm to obtain an alkalized activated acid solution; (4) performing solid-liquid separation on the alkalized activated acid solution in step (3) to obtain aluminum-calcium-rich detoxification activated acid solution and iron-chromium precipitate.
13. A calcium-aluminum-rich detoxification activation acid solution and iron-chromium precipitate prepared by the method according to any one of claims 1 to 12.
14. A use of the iron-chromium precipitate as claimed in claim 13, characterized in that: The ferrochromium slag is used for preparing smelting raw materials and ferrochromium alloy.