A high-solids-content, high-flash-point, odorless alkyd resin and its preparation method
By adjusting the ratio of fatty acids, polyols, polybasic acids and monobasic acids in alkyd resin, combined with multiple insulation reactions and the use of additives, the problems of solid content, odor and flash point of alkyd resin are solved, and high solidity is achieved Alkyd resin containing, high flash point and clean odor, suitable for a wider range of coatings and other applications.
Patent Information
- Application Number
- CN202211597005.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The existing alkyd resin has lower solid content, greater odor and lower flash point, which limits its application in coatings and other fields.
Prepare a specific proportion of synthetic fatty acids, polyols, polybasic acids and monobasic acids. Through multiple insulation reactions and the addition of additives, the acidity and solid content are reduced, the flash point is increased, and the esterification is controlled through specific alcohols and alcohol selection. Reaction rate and stability reduce small molecule acid anhydride residue and reduce odor.
Alkyd resins with high solid content, high flash point and clean odor are achieved, which meets higher application needs, and the flash point exceeds the national regulations of 60℃, avoiding inclusion in the scope of hazardous chemical management.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alkyd resin preparation, in particular to the field of IPCC08G63, and more specifically to an alkyd resin with high solid content, high flash point and no odor and a preparation method thereof. Background Art
[0002] In recent years, the preparation technology of alkyd resin in my country has become quite mature. With the continuous development of downstream industries such as coatings, curing agents, and adhesives, the demand for alkyd resin applications has also continued to expand, from 2.128 million tons in 2014 to 3.085 million tons in 2019, with an average annual compound growth rate of about 7.7%. However, the solid content of alkyd resin is low, the odor is strong, and the flash point is low, which limits the application of alkyd resin to a certain extent.
[0003] CN102952261A discloses an alkyd resin, a preparation method of an alkyd resin, and a three-dimensional network anticorrosive coating using an alkyd resin, and relates to an anticorrosive coating. The preparation method of the alkyd resin is as follows: a mixture of soybean oil, benzoic acid, and pentaerythritol is heated, and then yellow lead is added, alcoholyzed, and after cooling, phthalic anhydride and xylene are added to carry out esterification reaction, and then the product is pumped into a dilution tank to which gasoline has been added, and stirred to obtain an alkyd resin. However, the alkyd resin prepared by the invention has a high acid value (12 mg KOH / g), and the use of too much solvent reduces the solid content, which affects the application of the alkyd resin in the coating to a certain extent. Summary of the invention
[0004] In order to overcome the shortcomings of the background technology, the first aspect of the present invention provides a high-solid content, high-flash point and odorless alkyd resin, which comprises, by weight percentage, 25-35wt% of synthetic fatty acids, 10-18wt% of polyols, 5-10wt% of monobasic acids, 15-24wt% of polyacids, 0.5-2wt% of additives, and the balance is made up of solvents.
[0005] The synthetic fatty acid includes one or more of soybean oil fatty acid, safflower oil fatty acid, linseed oil fatty acid, dehydrated castor oil fatty acid and tung oil fatty acid.
[0006] Preferably, the acid value of the synthetic fatty acid is 160-220 mgKOH / g, and the iodine value of the synthetic fatty acid is 120-145 g I / 100 g.
[0007] Further preferably, the synthetic fatty acid is soybean oil fatty acid purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with an acid value of 201 mgKOH / g, and the iodine value of the synthetic fat is 141 g I / 100g.
[0008] The monoacid includes one or more of benzoic acid, abietic acid, linoleic acid, tall oil acid, soybean oil acid, rapeseed oil acid, coconut oil acid and ricinoleic acid.
[0009] Preferably, the monoacid comprises benzoic acid (CAS: 65-85-0), purchased from Jiangsu Sanmu Group Co., Ltd.
[0010] The polyacid includes one or more of phthalic anhydride, isophthalic acid, trimellitic anhydride, maleic anhydride and maleic anhydride.
[0011] The applicant has found that the polyacid includes phthalic anhydride, trimellitic anhydride and maleic anhydride. When the weight ratio of phthalic anhydride, trimellitic anhydride and maleic anhydride is 1:(0.1-0.3):(0.8-2), the acidity of the alkyd resin can be further reduced. The carboxyl reaction activity of phthalic anhydride and maleic anhydride is higher at 170°C. The three carboxyl groups of trimellitic anhydride have different reaction temperatures: the first carboxyl group is 150-170°C, the second carboxyl group is 175-190°C, and the third carboxyl group is 210-220°C. According to the different reactivity of the three carboxyl groups, a specific insulation reaction program is selected in the preparation process, the temperature of the first insulation reaction is 175-185°C, the temperature of the second insulation reaction is 195-205°C, the temperature of the third insulation reaction is 205-210°C, the temperature of the fourth insulation reaction is 215-225°C, and the temperature of the fifth insulation reaction is 230-240°C, so that the carboxyl activity corresponds to the insulation reaction temperature, thereby reducing the acidity of the alkyd resin. Due to the more complete reaction, the residual small molecule acid anhydride is reduced, and the odor of the alkyd resin is further reduced.
[0012] Preferably, the polyacid comprises phthalic anhydride, trimellitic anhydride and maleic anhydride, and the weight ratio of phthalic anhydride, trimellitic anhydride and maleic anhydride is 1:(0.1-0.3):(0.8-2).
[0013] Further preferably, the polyacid includes phthalic anhydride (CAS: 85-44-9), trimellitic anhydride (CAS: 552-30-7) and maleic anhydride (CAS: 108-31-6), and the weight ratio of phthalic anhydride, trimellitic anhydride and maleic anhydride is 1:0.1:0.9.
[0014] Preferably, the weight ratio of the synthetic fatty acid to the polyol is 1:(0.4-0.6).
[0015] Further preferably, the weight ratio of the synthetic fatty acid to the polyol is 1:0.5.
[0016] Preferably, the weight ratio of the monoacid to the polyacid is 1:(2-3).
[0017] Further preferably, the weight ratio of the monoacid to the polyacid is 1:2.5.
[0018] The functionality of the polyol is 2-5, and the hydroxyl content of the polyol is 30-55 wt%.
[0019] The applicant has found that the acid value of the prepared alkyd resin can be reduced by compounding triols and tetraols as polyols. It is speculated that alcohols with different functionalities can control the rate of esterification reaction and make the esterification reaction proceed smoothly. Further research has found that when the tetraol is pentaerythritol, the triol is trimethylolpropane, and the weight ratio of pentaerythritol to trimethylolpropane is 1: (0.8-1.8), not only the reaction rate can be controlled, but also the solid content of the alkyd resin can be increased. This may be because pentaerythritol has four primary hydroxyl groups, has a large functionality and high activity, which can increase the reaction rate. However, when the content of pentaerythritol is too high, it is easy to cause the viscosity to rise too fast in the later stage of esterification, and the reaction is difficult to control, and even gelation occurs. Adding an appropriate proportion of trimethylolpropane can reduce the occurrence of gelation. It may be that trimethylolpropane has three primary hydroxyl groups and one alkyl branched chain, which is less than pentaerythritol in functionality and has relatively weak reaction activity. At the same time, the alkyl side chain of trimethylolpropane can reduce the interaction between the three primary hydroxyl groups, improve the miscibility of alkyd resin and solvent, and thus increase the solid content.
[0020] Preferably, the polyol comprises triol and tetraol, and the weight ratio of the triol to the tetraol is 1:(0.8-1.8).
[0021] Further preferably, the polyol includes triol and tetraol, and the weight ratio of the triol to the tetraol is 1:1.5.
[0022] Preferably, the triol includes trimethylolpropane (CAS: 77-99-6).
[0023] Preferably, the tetrahydric alcohol includes pentaerythritol (CAS: 115-77-5).
[0024] Further preferably, the tetrahydric alcohol includes pentaerythritol (CAS: 115-77-5), which is purchased from Jinan Haobang Chemical Co., Ltd., has a hydroxyl content of 48.5 wt%, and is of grade 98.
[0025] The auxiliary agent includes one or more of magnesium oxide, calcium oxide, lithium hydroxide, sodium hydride, potassium hydride, sodium hydroxide, and potassium hydroxide.
[0026] Preferably, the auxiliary agent comprises lithium hydroxide (CAS: 1310-65-2).
[0027] Preferably, the solvent comprises o-xylene (CAS: 95-47-6).
[0028] The second aspect of the present invention provides a method for preparing a high-solid content, high-flash point, and odor-free alkyd resin, comprising the following steps:
[0029] S1, adding synthetic fatty acid, polyol, monobasic acid, polybasic acid, and solvent in sequence, stirring after heating, and adding auxiliary agent to react;
[0030] S2, sequentially performing the first heat preservation reaction, the second heat preservation reaction, the third heat preservation reaction, and the fourth heat preservation reaction, and testing the acid value to be 25-35 mgKOH / g;
[0031] S3, the fifth heat preservation reaction
[0032] S4, cooling, diluting, filtering and packaging to obtain the alkyd resin.
[0033] The temperature of the first insulation reaction is 175-185°C, the temperature of the second insulation reaction is 195-205°C, the temperature of the third insulation reaction is 205-210°C, the temperature of the fourth insulation reaction is 215-225°C, and the temperature of the fifth insulation reaction is 230-240°C.
[0034] Preferably, the temperature of the first insulation reaction is 180°C, the temperature of the second insulation reaction is 200°C, the temperature of the third insulation reaction is 210°C, the temperature of the fourth insulation reaction is 220°C, and the temperature of the fifth insulation reaction is 235°C.
[0035] The first insulation reaction time is 0.5-1h, the second insulation reaction time is 0.5-1h, the third insulation reaction time is 0.5-1h, the fourth insulation reaction time is 0.4-0.7h, and the fifth insulation reaction time is 0.2-0.5h.
[0036] Preferably, the first insulation reaction time is 1 hour, the second insulation reaction time is 1 hour, the third insulation reaction time is 0.5 hour, the fourth insulation reaction time is 0.4 hour, and the fifth insulation reaction time is 0.3 hour.
[0037] Preferably, the acid value of the alkyd resin is 7-12 mg KOH / g; and the viscosity (25° C.) of the alkyd resin is 20-25 s.
[0038] Beneficial effects:
[0039] 1. The acid value of the prepared alkyd resin can be reduced by compounding triols and tetraols. It is speculated that alcohols with different functionalities can control the rate of the esterification reaction and make the esterification reaction proceed smoothly.
[0040] 2. When the tetrahydric alcohol is pentaerythritol, the trihydric alcohol is trimethylolpropane, and the weight ratio of pentaerythritol to trimethylolpropane is 1:(0.8-1.8), not only the reaction rate can be controlled, but also the solid content of the alkyd resin can be increased.
[0041] 3. The polyacid includes phthalic anhydride, trimellitic anhydride and maleic anhydride. When the weight ratio of phthalic anhydride, trimellitic anhydride and maleic anhydride is 1:(0.1-0.3):(0.8-2), the acidity of the alkyd resin can be further reduced.
[0042] 4. The resin made in the present invention has a high flash point, which exceeds the national standard of 60°C and is not included in the category of hazardous chemicals management. DETAILED DESCRIPTION
[0043] Example 1
[0044] The invention discloses an alkyd resin with high solid content, high flash point and no odor. The components thereof include, by weight percentage, 32 wt% synthetic fatty acid, 16 wt% polyol, 8 wt% monoacid, 20 wt% polyacid, 1 wt% auxiliary agent and the balance made up by solvent.
[0045] The synthetic fatty acid is soybean oil fatty acid purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with an acid value of 201 mgKOH / g, and the iodine value of the synthetic fat is 141 g I / 100 g.
[0046] The polyol includes triol and tetraol, and the weight ratio of the triol to the tetraol is 1:1.5.
[0047] The triol includes trimethylolpropane (CAS: 77-99-6).
[0048] The tetrahydric alcohol includes pentaerythritol (CAS: 115-77-5), which is purchased from Jinan Haobang Chemical Co., Ltd., has a hydroxyl content of 48.5 wt %, and is model: 98 grade.
[0049] The monoacid includes benzoic acid (CAS: 65-85-0), which was purchased from Jiangsu Sanmu Group Co., Ltd.
[0050] The polyacid comprises phthalic anhydride (CAS: 85-44-9), trimellitic anhydride (CAS: 552-30-7) and maleic anhydride (CAS: 108-31-6), and the weight ratio of the phthalic anhydride, trimellitic anhydride and maleic anhydride is 1:0.1:0.9.
[0051] The auxiliary agent includes lithium hydroxide (CAS: 1310-65-2).
[0052] The solvent includes o-xylene (CAS: 95-47-6).
[0053] A method for preparing a high-solid content, high-flash point, and odor-free alkyd resin comprises the following steps:
[0054] S1, add synthetic fatty acid, polyol, monobasic acid, polybasic acid, and solvent in sequence, heat to 120°C and stir until dissolved, heat to 150°C and add auxiliary agent and continue reaction for 2h;
[0055] S2, sequentially performing the first heat preservation reaction, the second heat preservation reaction, the third heat preservation reaction, and the fourth heat preservation reaction, and the acid value is tested to be 30 mgKOH / g;
[0056] S3, performing the fifth heat preservation reaction;
[0057] S4, cooling to 160°C, diluting, filtering and packaging to obtain the alkyd resin.
[0058] The temperature of the first insulation reaction is 180°C, the temperature of the second insulation reaction is 200°C, the temperature of the third insulation reaction is 210°C, the temperature of the fourth insulation reaction is 220°C, and the temperature of the fifth insulation reaction is 235°C.
[0059] The first insulation reaction time is 1 hour, the second insulation reaction time is 1 hour, the third insulation reaction time is 0.5 hour, the fourth insulation reaction time is 0.4 hour, and the fifth insulation reaction time is 0.3 hour.
[0060] The acid value and viscosity (25° C.) of the alkyd resin are shown in Table 1.
[0061] Example 2
[0062] The specific implementation is the same as that of Example 1; the difference is that the weight ratio of phthalic anhydride, trimellitic anhydride and maleic anhydride in Example 2 is 1:0.15:1.5.
[0063] Comparative Example 1
[0064] The specific implementation is the same as Example 1; the difference is that the polyacid in Comparative Example 1 includes phthalic anhydride (CAS: 85-44-9) and maleic anhydride (CAS: 108-31-6), and the weight ratio of phthalic anhydride to maleic anhydride is 1:0.9.
[0065] Comparative Example 2
[0066] The specific implementation is the same as Example 1; the difference is that the weight ratio of phthalic anhydride, trimellitic anhydride and maleic anhydride in Comparative Example 2 is 1:0.3:2.5.
[0067] Comparative Example 3
[0068] The specific implementation is the same as Example 1; the difference is that the weight ratio of pentaerythritol to trimethylolpropane in Comparative Example 3 is 1:2.
[0069] Performance Testing Methods
[0070] The alkyd resins prepared in the examples and comparative examples were subjected to the following tests, and the test data are listed in Table 1.
[0071] 1. Solid content test: Measure by drying method. Use analytical balance to accurately weigh 2g alkyd resin and dry it in an oven at 103°C for 4 hours. The mass of the sample after drying is m1. Solid content (%) = (2-m1) / 2*100%.
[0072] 2. Acid value test: Test according to the provisions of Method A "Partial Acid Value" in GB / T 6743-2008.
[0073] 3. Flash point test: Refer to GB / T261-2008 standard and use Pensky-Martin closed cup to measure the flash point of alkyd resin.
[0074] 4. Viscosity test: Grignard tube viscometer operation steps: Pour the sample into the viscosity tube, about to the 100mm mark, plug it, and put it in 25℃ water. After 10 minutes, adjust the liquid level to exactly 100mm, plug it to the 108mm mark, and continue to put it in a 25℃ constant temperature water bath. After 10 minutes, quickly invert the viscosity tube, and place the viscosity tube vertically in a 25℃ water bath to measure the time required for the bubble to rise to the top of the viscosity tube.
[0075] 5. Odor rating test: Odor rating was determined by sensory evaluation similar to the VDA270 test procedure. The detailed steps are as follows. At 25°C, 10 g of alkyd resin was placed in a 1 liter glass vial for sensory evaluation. The sensory evaluation was conducted by 15 trained functional inspectors who provided odor ratings based on the ratings described below. The reported results are the average ratings of the functional inspectors.
[0076] Rating description: 1 Not noticeable; 2 Noticeable, but not disturbing; 3 Clearly noticeable, but not disturbing; 4 Disturbing; 5 Strongly disturbing; 6 Unacceptable.
[0077] Performance test data
[0078] Table 1
[0079] Solid content (%) Acid value (mgKOH / g) Flash point(℃) Viscosity(s) Odor level Example 1 78 7 62 22 2 Example 2 76 8 62 24 2 Comparative Example 1 68 16 58 32 3 Comparative Example 2 70 13 60 28 3 Comparative Example 3 71 14 59 30 3
Claims
1. A high solid content, high flash point, clean alkyd resin, characterized in that: The components include, by weight percentage: 25-35wt% synthetic fatty acid, 10-18wt% polyol, 5-10wt% monoacid, 15-24wt% polyacid, 0.5-2wt% auxiliary agent, and the balance is made up of solvent; The polyol includes a triol and a tetraol, the triol includes trimethylolpropane, the tetraol includes pentaerythritol, and the weight ratio of the triol to the tetraol is 1:1.5; The polyacid comprises phthalic anhydride, trimellitic anhydride and maleic anhydride, and the weight ratio of the phthalic anhydride, trimellitic anhydride and maleic anhydride is 1:(0.1-0.3):(0.8-2).
2. The high-solid, high-flash-point, clean alkyd resin according to claim 1, characterized in that: The acid value of the synthetic fatty acid is 160-220 mg KOH / g, and the iodine value of the synthetic fatty acid is 120-145 gI / 100 g.
3. The high-solid, high-flash-point, clean alkyd resin according to claim 1, characterized in that: The weight ratio of the synthetic fatty acid to the polyol is 1:(0.4-0.6).
4. The high-solid, high-flash-point, clean alkyd resin according to claim 1, characterized in that: The weight ratio of the monoacid to the polyacid is 1:(2-3).
5. A method for preparing a high-solid content, high-flash point, clean alkyd resin according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, adding synthetic fatty acid, polyol, monobasic acid, polybasic acid, and solvent in sequence, stirring after heating, and adding auxiliary agent to react; S2, sequentially performing the first heat preservation reaction, the second heat preservation reaction, the third heat preservation reaction, and the fourth heat preservation reaction, and testing the acid value to be 25-35 mg KOH / g; S3, performing the fifth heat preservation reaction; S4, cooling, diluting, filtering and packaging to obtain the alkyd resin.
6. The method for preparing a high-solid content, high-flash point, clean alkyd resin according to claim 5, characterized in that: The temperature of the first insulation reaction is 175-185°C, the temperature of the second insulation reaction is 195-205°C, the temperature of the third insulation reaction is 205-210°C, the temperature of the fourth insulation reaction is 215-225°C, and the temperature of the fifth insulation reaction is 230-240°C.
7. The method for preparing a high-solid content, high-flash point, clean alkyd resin according to claim 6, characterized in that: The acid value of the alkyd resin is 7-12 mg KOH / g; the viscosity of the alkyd resin is 20-25 s.
Citation Information
Patent Citations
Alkyd resin, preparation method of alkyd resin and three-dimensional network anticorrosive coating using alkyd resin
CN102952261A
Functional resin for paint and manufacture method thereof
CN101245132A
Epoxy-modified waterborne alkyd resin and preparation method thereof
CN105504246A
Odorless alkyd resin and preparation method thereof
CN106349463A
High-solid-content low-viscosity low-hydroxyl-value low-dilution-rate alkyd resin, and preparation method and applications thereof
CN108822285A