Ultra-light and highly flame-retardant biodegradable PLA foam and its preparation process
Through the chain extension modification of PLA and PBAT and the synergistic use of flame retardants, combined with the supercritical foaming process, the problem of flammability of PLA foam is solved, and the efficient preparation of PLA foam with low density and good flame retardant properties is achieved, which is suitable for Various application scenarios.
Patent Information
- Application Number
- CN202211548273.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing PLA foam materials are flammable and have insufficient flame retardant properties, making it difficult to prepare PLA flame retardant foam materials with low density and good flame retardant effects.
PLA and PBAT are chain extended and modified using an epoxy chain extender, combined with lignin, ammonium polyphosphate and resorcinol-bis(diphenyl phosphate) condensation polymer (RDP) as a flame retardant system, and in supercritical Foaming is carried out under carbon dioxide atmosphere, and silica aerogel is selected as the foaming nucleating agent to improve the melt strength and flame retardant properties of the material.
Ultra-light and highly flame-retardant biodegradable PLA foam with low density, low thermal conductivity and good flame retardancy has been obtained, which is suitable for packaging, insulation and shock absorption and other fields.
Smart Images

Figure SMS_1 
Figure HDA0003981047670000011 
Figure HDA0003981047670000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PLA foam, and in particular to an ultra-light and highly flame-retardant biodegradable PLA foam and a preparation process thereof. Background Art
[0002] Polylactic acid (PLA) is one of the most widely used biodegradable materials in recent years. Preliminary studies have demonstrated the advantages and potential of PLA foam materials in thermal insulation applications, but most polymer foam materials have a fatal disadvantage - flammability. In real fire scenarios, most unmodified polymers will burn violently. PLA, as a typical linear aliphatic polyester, will burn with a large number of molten droplets and release a large amount of heat and smoke. In order to further expand the application scenarios of PLA foam, people have conducted a lot of research on improving the flame retardant properties of PLA. At present, the flame retardant modification of PLA and its composites is mainly based on the following three methods: 1) chemical grafting to modify the PLA molecular chain; (2) melt blending and adding flame retardants to prepare flame-retardant PLA composites; (3) surface treatment of PLA and its composites.
[0003] At present, the following methods are mainly used to prepare PLA flame retardant materials: (1) Halogen flame retardants played an important role in the early stage of research on PLA flame retardant materials. They have advantages such as good flame retardant effect, low addition amount, and little effect on the mechanical energy absorption of the material, which is unmatched by other flame retardants. However, they produce harmful gases such as hydrogen halide during high-temperature combustion, which limits their application. (2) Metal hydroxides are also commonly used as flame retardants for polymers. They absorb heat and dehydrate during combustion to prevent the polymer from heating up. At the same time, they release water vapor to dilute the oxygen concentration and form a metal oxide flame retardant layer on the polymer surface. However, they require a very high load to achieve good flame retardancy. (3) Recent studies have found that the addition of a small amount of nanoparticles can improve the charring ability of PLA after combustion to varying degrees and avoid the droplet phenomenon during PLA combustion. Adding inorganic nanomaterials to polylactic acid and its composites as key flame retardant materials can not only meet the required industrial flame retardant requirements, but also maintain or even improve the excellent properties of polylactic acid. Phosphorus and nitrogen flame retardants are environmentally friendly, such as phosphate flame retardants and ammonium polyphosphate (APP). They have been highly popular in recent years due to their good flame retardant effects, low prices, readily available raw materials, and simple and convenient processing.
[0004] Although researchers have conducted a lot of research on PLA flame-retardant composite materials, there are few studies on PLA flame-retardant foam materials. This is because the inherent melt strength of polylactic acid is low, and it is difficult to prepare low-density foams. The introduction of a large amount of flame-retardant fillers seriously reduces the melt strength, which is not conducive to the preparation of foaming materials. Although the melt strength of PLA can be improved by modification, it does not have a good flame retardant effect.
[0005] PLA and PBAT have great potential for use as biodegradable raw materials throughout their life cycle, but at the same time, the performance of the materials must be taken into account, such as thermal insulation, which can reduce energy dissipation, and flame retardancy, which can ensure life safety. Therefore, functional biodegradable materials will have broad application prospects. Therefore, we must not only study how to improve the melt strength of PLA and PBAT and reduce the foaming density of the materials, but also study functional foaming materials and the synergistic effect of different flame retardants to obtain ultra-light, flame-retardant, and heat-insulating fully biodegradable foam materials. Summary of the invention
[0006] The present invention aims to solve the above technical problems and provide a foam material which is ultra-light, flame-retardant and fully biodegradable and can be used in various fields such as heat preservation, packaging and shock absorption.
[0007] An embodiment of the present invention provides a preparation process of an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0008] Step S1, mixing RDP and ethanol and stirring evenly to obtain an RDP ethanol dispersion, putting lignin, APP and silica aerogel into a container, mixing and stirring evenly to obtain a flame retardant mixture, spraying the RDP ethanol dispersion evenly on the surface of the flame retardant blend, stirring evenly, and waiting for the ethanol to evaporate completely to obtain a flame retardant system;
[0009] Step S2, adding PLA and PBAT into a torque rheometer, and sequentially adding a flame retardant system and an epoxy chain extender for mixing, and obtaining a mixed sample after the reaction is completed;
[0010] Step S3, placing the mixed sample into a molding device for molding to obtain a molded sample;
[0011] Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming under a carbon dioxide atmosphere to obtain a foamed sample;
[0012] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0013] In the above technical scheme, epoxy chain extender is selected to extend and modify PLA and PBAT to improve the melt strength and foaming performance of the material, thereby obtaining a low-density foam material; lignin / APP / RDP synergistic system or lignin / APP / RDP / silicon dioxide gas condensation synergistic system is selected as the flame retardant system. PLA and PBAT are biodegradable and environmentally friendly materials, so environmentally friendly flame retardants should also be selected. Lignin is a biopolymer with a three-dimensional network structure. It is the second most abundant organic matter in nature and contains rich aromatic ring structures, aliphatic and aromatic hydroxyl groups, and quinone groups and other active groups. Therefore, lignin is a high-quality choice as a carbon source for an intumescent flame retardant system. Ammonium polyphosphate (APP) is a commonly used wood flame retardant, which can be used as an acid source for an intumescent flame retardant system. It can generate ammonia and a very stable polyphosphoric acid by thermal decomposition during the combustion process, and can generate a carbon layer on the surface of the polymer to isolate oxygen. Resorcinol-bis(diphenyl phosphate) condensation polymer (RDP) is a liquid, highly efficient, halogen-free, environmentally friendly flame retardant plasticizer with a polyphosphate structure. After being first blended with lignin and APP, it can cover a layer on the surface of lignin and APP, thereby increasing the interfacial compatibility of the two flame retardants with the polymer and further improving the flame retardant properties of the material; silica aerogel particles in the system can not only act as a foaming nucleating agent, but also have a certain insulation and smoke suppression effect. The intermittent supercritical carbon dioxide foaming process is used to obtain PLA foam with ultra-low density and high flame retardant properties.
[0014] In a specific embodiment, in step S1, the mass ratio of RDP to ethanol is 1:10, RDP is 1-1.5 parts by mass; lignin is 3-5 parts by mass; APP is 14-20 parts by mass; and silica aerogel is 0-3 parts by mass.
[0015] In a specific embodiment, in step S2, the epoxy chain extender is ADR or TGIC.
[0016] In a specific embodiment, in step S2, the reaction temperature is 190-210° C. and the reaction time is 10 min.
[0017] In a specific embodiment, in step S3, the molding device is a flat plate vulcanizer, and the mixed sample is placed in a mold of the flat plate vulcanizer, and hot pressing is performed at 180-195°C and 10 MPa for 3 minutes and then cold pressing is performed for 5 minutes to obtain a plate-shaped molded sample.
[0018] In a specific embodiment, in step S3, the molding device is a crusher, the mixed sample is placed in the crusher to be crushed into small particles, and then placed in an extruder for extrusion and granulation to obtain a granular molded sample.
[0019] In a specific embodiment, in step S4, the supercritical reaction temperature is 130-140° C., the pressure is 18-30 MPa, and the saturation time is 2-6 h.
[0020] An embodiment of the present invention provides an ultra-light and highly flame-retardant biodegradable PLA foam, which is prepared by using the above-mentioned preparation process of the ultra-light and highly flame-retardant biodegradable PLA foam.
[0021] Compared with the prior art, the present invention has the following beneficial technical effects:
[0022] 1. Use epoxy chain extender to extend and modify PLA and PBAT to improve the melt strength and foaming performance of the material, thereby obtaining a low-density PLA foam material with stable structure;
[0023] 2. Select the lignin / APP / RDP / silicon dioxide aerosol synergistic system as the flame retardant system to improve the flame retardant properties of the material;
[0024] 3. Adopt intermittent supercritical carbon dioxide foaming process to obtain PLA foam with ultra-low density and high flame retardancy;
[0025] The PLA foam prepared by the present invention has low density, low thermal conductivity, good flame retardancy, and is fully biodegradable, and can be widely used in packaging, thermal insulation, and shock absorption fields such as express packaging, cold chain packaging, vaccine packaging, exterior wall insulation, and interior decoration. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is an electron microscope image of the cell structure of Example 1;
[0027] Figure 2 This is an electron microscope image of the cell structure of Example 2;
[0028] Figure 3 This is an electron microscope image of the cell structure of Example 3;
[0029] Figure 4 This is an electron microscope image of the cell structure of Example 4;
[0030] Figure 5 This is an electron microscope image of the cell structure of Example 5;
[0031] Figure 6 This is an electron microscope image of the cell structure of Comparative Example 1;
[0032] Figure 7 This is an electron microscope image of the cell structure of Comparative Example 2;
[0033] Figure 8 This is an electron microscope image of the cell structure of Comparative Example 3;
[0034] Fig. 9This is an electron microscope image of the cell structure of Comparative Example 4;
[0035] Fig.10 This is a digital photo of the carbon residue after the foam material in Example 2 was subjected to a cone calorimetry test;
[0036] Fig.11 This is a digital photo of the carbon residue after the foam material in Example 3 was subjected to a cone calorimetry test;
[0037] Fig.12 This is a digital photo of the carbon residue after the foam material in Comparative Example 1 was subjected to a cone calorimetry test;
[0038] Fig.13 This is a digital photo of the carbon residue after the foamed material in Comparative Example 4 was subjected to a cone calorimetry test. DETAILED DESCRIPTION
[0039] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0040] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0041] Example 1
[0042] This embodiment prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0043] Step S1, 1 part by mass of RDP and 10 parts by mass of ethanol are mixed and stirred to obtain an RDP ethanol dispersion, 5 parts by mass of lignin and 14 parts by mass of APP are put into a container, mixed and stirred to obtain a flame retardant mixture, and the RDP ethanol dispersion is evenly sprayed on the surface of the flame retardant blend, stirred evenly, and the ethanol is evaporated to obtain a flame retardant system;
[0044] Step S2, adding 95 parts by mass of PLA and 5 parts by mass of PBAT into a torque rheometer, and sequentially adding 20 parts by mass of a flame retardant system and 1 part by mass of ADR for mixing, reacting at 200° C. for 8 minutes, and obtaining a mixed sample after the reaction is completed;
[0045] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 185° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0046] Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming at 140° C. and 20 MPa of carbon dioxide atmosphere for 5 hours to obtain a foamed sample;
[0047] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0048] Example 2
[0049] This embodiment prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0050] Step S1, 1 part by mass of RDP and 10 parts by mass of ethanol are mixed and stirred to obtain an RDP ethanol dispersion, 5 parts by mass of lignin and 19 parts by mass of APP are put into a container, mixed and stirred to obtain a flame retardant mixture, and the RDP ethanol dispersion is evenly sprayed on the surface of the flame retardant blend, stirred evenly, and the ethanol is evaporated to obtain a flame retardant system;
[0051] Step S2, adding 90 parts by mass of PLA and 10 parts by mass of PBAT into a torque rheometer, and sequentially adding 25 parts by mass of a flame retardant system and 2 parts by mass of ADR for mixing, reacting at 200° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0052] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 190° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0053] Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming for 4 hours at 130° C. and 23 MPa of carbon dioxide atmosphere to obtain a foamed sample;
[0054] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0055] Example 3
[0056] This embodiment prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0057] Step S1, 1 part by mass of RDP and 10 parts by mass of ethanol are mixed and stirred to obtain an RDP ethanol dispersion, 5 parts by mass of lignin, 18 parts by mass of APP and 1 part by mass of silica aerogel are put into a container, mixed and stirred to obtain a flame retardant mixture, the RDP ethanol dispersion is evenly sprayed on the surface of the flame retardant blend, stirred evenly, and the ethanol is evaporated to obtain a flame retardant system;
[0058] Step S2, adding 85 parts by mass of PLA and 15 parts by mass of PBAT into a torque rheometer, and sequentially adding 25 parts by mass of a flame retardant system and 2 parts by mass of ADR for mixing, reacting at 210° C. for 8 minutes, and obtaining a mixed sample after the reaction is completed;
[0059] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 195° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0060] Step S4, placing the molded sample in a supercritical reactor, and performing supercritical foaming at 130° C. and 25 MPa of carbon dioxide atmosphere for 3 hours to obtain a foamed sample;
[0061] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0062] Example 4
[0063] This embodiment prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0064] Step S1, 1 part by mass of RDP and 10 parts by mass of ethanol are mixed and stirred to obtain an RDP ethanol dispersion, 3 parts by mass of lignin, 18 parts by mass of APP and 3 parts by mass of silica aerogel are put into a container, mixed and stirred to obtain a flame retardant mixture, and the RDP ethanol dispersion is evenly sprayed on the surface of the flame retardant blend, stirred evenly, and the ethanol is evaporated to obtain a flame retardant system;
[0065] Step S2, adding 95 parts by mass of PLA and 5 parts by mass of PBAT into a torque rheometer, adding 25 parts by mass of a flame retardant system and 1.5 parts by mass of ADR in sequence for mixing, reacting at 200° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0066] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 185° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0067] Step S4, placing the molded sample in a supercritical reactor, and performing supercritical foaming for 6 hours at 140° C. and 20 MPa of carbon dioxide atmosphere to obtain a foamed sample;
[0068] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0069] Example 5
[0070] This embodiment prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0071] Step S1, 1.5 parts by mass of RDP and 15 parts by mass of ethanol are mixed and stirred to obtain an RDP ethanol dispersion, 4 parts by mass of lignin, 18 parts by mass of APP and 1.5 parts by mass of silica aerogel are put into a container, mixed and stirred to obtain a flame retardant mixture, and the RDP ethanol dispersion is evenly sprayed on the surface of the flame retardant blend, stirred evenly, and the ethanol is evaporated to obtain a flame retardant system;
[0072] Step S2, adding 80 parts by mass of PLA and 20 parts by mass of PBAT into a torque rheometer, and sequentially adding 25 parts by mass of a flame retardant system and 2 parts by mass of ADR for mixing, reacting at 200° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0073] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 185° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0074] Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming at 140° C. and 25 MPa of carbon dioxide atmosphere for 5 hours to obtain a foamed sample;
[0075] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0076] Comparative Example 1
[0077] This comparative example prepares an ultra-light biodegradable PLA foam, comprising the following steps:
[0078] Step S1, adding 100 parts by mass of PLA into a torque rheometer, adding 1 part by mass of ADR for mixing, reacting at 200° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0079] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 180° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0080] Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming for 4 hours at 130° C. and 20 MPa of carbon dioxide atmosphere to obtain a foamed sample;
[0081] Step S5: Cooling and shaping the foamed sample to obtain ultra-light biodegradable PLA foam.
[0082] Comparative Example 2
[0083] This comparative example prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0084] Step S1, putting 20 parts by mass of APP into a container to obtain a flame retardant system;
[0085] Step S2, adding 100 parts by mass of PLA into a torque rheometer, adding 20 parts by mass of a flame retardant system and 1 part by mass of ADR in sequence for mixing, reacting at 200° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0086] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 180° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0087] Step S4, placing the molded sample in a supercritical reactor, and performing supercritical foaming for 4 hours at 130° C. and 18 MPa of carbon dioxide atmosphere to obtain a foamed sample;
[0088] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0089] Comparative Example 3
[0090] This comparative example prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0091] Step S1, putting 20 parts by mass of lignin into a container to obtain a flame retardant system;
[0092] Step S2, adding 95 parts by mass of PLA and 5 parts by mass of PBAT into a torque rheometer, adding 20 parts by mass of a flame retardant system and 1.5 parts by mass of ADR in sequence for mixing, reacting at 200° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0093] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 180° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0094] Step S4, placing the molded sample in a supercritical reactor, and performing supercritical foaming for 6 hours at 140° C. and 20 MPa of carbon dioxide atmosphere to obtain a foamed sample;
[0095] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0096] Comparative Example 4
[0097] This comparative example prepares an ultra-light and highly flame-retardant biodegradable PLA foam, comprising the following steps:
[0098] Step S1, putting 5 parts by mass of lignin and 15 parts by mass of APP into a container, mixing and stirring to obtain a flame retardant system;
[0099] Step S2, adding 95 parts by mass of PLA and 5 parts by mass of PBAT into a torque rheometer, and sequentially adding 25 parts by mass of a flame retardant system and 1 part by mass of ADR for mixing, reacting at 190° C. for 10 minutes, and obtaining a mixed sample after the reaction is completed;
[0100] Step S3, placing the mixed sample in a flat vulcanizing machine mold, hot pressing for 3 minutes at 185° C. and 10 MPa, and then cold pressing for 5 minutes to obtain a plate-shaped molded sample;
[0101] Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming at 130° C. and 20 MPa of carbon dioxide atmosphere for 5 hours to obtain a foamed sample;
[0102] Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
[0103] Performance Testing
[0104] 1. Density: Tested according to ASTM D 792;
[0105] 2. Thermal conductivity test: using Hot Disk thermal constant analyzer (TPS 2500S);
[0106] 3. Oxygen index: tested according to GB / T2406.2-2009;
[0107] 4. Ignition time, peak heat release rate and total smoke production are tested by cone calorimeter according to ISO5660-1993 standard;
[0108] 5. Vertical burning: Tested according to standard ASTM D3801-10.
[0109] The foam materials obtained in Examples 1-5 and Comparative Examples 1-4 were tested for performance. The results are shown in Table 1.
[0110] Table 1 Foam material performance test
[0111]
[0112] As can be seen from Table 1, in Comparative Example 1, the heat release rate of the PLA foam without adding flame retardant is extremely high during combustion, which will cause the fire to spread rapidly in an actual fire, which is a very dangerous phenomenon. In Comparative Examples 2-4, the heat release rate of the PLA foam modified with lignin fiber and / or APP is significantly reduced, because the two form a thick carbon layer on the surface of the material, but the continuous burning time is still maintained at more than 930s during the entire combustion process.
[0113] In Examples 1 to 5, a phosphorus-based flame retardant RDP is introduced into the flame retardant system. The phosphorus-based flame retardant can be thermally decomposed during combustion to produce phosphorus-containing oxygen acids, which can promote the dehydration and carbonization of hydroxyl-containing organic matter (for example, PLA and lignin fiber) to produce a char layer on the surface. The oxygen index of the char layer is much higher than that of the organic matter, which can isolate the combustibles from oxygen and separate the flame from the combustibles. Most of the phosphorus elements in the flame retardant are gathered in the condensed phase to protect the char layer generated by combustion, preventing it from being oxidized into carbon dioxide by subsequent combustion, so that the continuous combustion time is reduced to about 830 seconds during the entire combustion process.
[0114] In Example 3-5, silica aerogel is introduced into the flame retardant system. The silica aerogel is continuously accumulated in the carbon residue during the combustion process, which can enhance the structural strength of the carbon residue and prolong the ignition time to more than 20 seconds.
[0115] Combined with Figure 10-13 After the PLA foam in Comparative Example 1 is burned, almost no carbon layer remains. After the PLA foam in Comparative Example 4 is burned, there is an obvious thick carbon layer. During the combustion process, the carbon layer is quickly generated and then slowly destroyed by the subsequent combustion. This process of generation and destruction is constantly cyclical, so the combustion process is prolonged but the combustion cannot be completely stopped. The residual carbon samples of the PLA foam in Examples 2 and 3 are more complete and have a denser structure.
[0116] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.
Claims
1. A process for preparing ultra-light and highly flame-retardant biodegradable PLA foam, characterized in that: The following steps are involved: Step S1, mixing RDP and ethanol to obtain RDP ethanol dispersion, putting lignin, APP and silica aerogel into a container, mixing and stirring to obtain a flame retardant mixture, spraying the RDP ethanol dispersion evenly on the surface of the flame retardant blend, stirring evenly, and waiting for the ethanol to evaporate to obtain a flame retardant system; the mass ratio of RDP to ethanol is 1:10, RDP is 1-1.5 parts by mass; lignin is 3-5 parts by mass; APP is 14-20 parts by mass; and silica aerogel is 0-3 parts by mass; Step S2, adding PLA and PBAT into a torque rheometer, and sequentially adding a flame retardant system and an epoxy chain extender for mixing, and obtaining a mixed sample after the reaction is completed; the epoxy chain extender is ADR or TGIC; Step S3, placing the mixed sample into a molding device for molding to obtain a molded sample; Step S4, placing the molded sample into a supercritical reactor, and performing supercritical foaming under a carbon dioxide atmosphere to obtain a foamed sample; Step S5, cooling and shaping the foamed sample to obtain ultra-light and highly flame-retardant biodegradable PLA foam.
2. The preparation process of an ultra-light and highly flame-retardant biodegradable PLA foam according to claim 1, characterized in that: In step S2, the reaction temperature is 190-210° C. and the reaction time is 10 min.
3. The preparation process of the ultra-light and highly flame-retardant biodegradable PLA foam according to claim 1, characterized in that: In step S3, the molding device is a flat plate vulcanizer, and the mixed sample is placed in a mold of the flat plate vulcanizer, and hot pressing is performed at 180-195° C. and 10 MPa for 3 minutes and then cold pressing is performed for 5 minutes to obtain a plate-shaped molded sample.
4. The process for preparing an ultra-light and highly flame-retardant biodegradable PLA foam according to claim 1, characterized in that: In step S3, the molding device is a crusher, the mixed sample is placed in the crusher to be crushed into small particles, and then placed in an extruder for extrusion and granulation to obtain a granular molded sample.
5. The process for preparing an ultra-light and highly flame-retardant biodegradable PLA foam according to claim 1, characterized in that: In step S4, the supercritical reaction temperature is 130-140° C., the pressure is 18-30 MPa, and the saturation time is 2-6 h.
6. An ultra-light and highly flame-retardant biodegradable PLA foam, characterized in that: The foam is prepared by the preparation process of the ultra-light and highly flame-retardant biodegradable PLA foam according to any one of claims 1 to 5.
Citation Information
Patent Citations
Polylactic acid nanometer bubble hole foaming material and preparation method thereof
CN109354847A
Polylactic acid / PBAT / thermoplastic starch composite foaming flame-retardant material and preparation method thereof
CN112898753A
Process for the preparation of hydroxyphosphonates and their use as flame retardants in polymers
EP0908464A1
Cited By
A biodegradable foam box for cold chain logistics and its preparation method
CN120554716B
Degradable material for making shoe soles
CN122790390A