Aluminum-scandium alloy target material and preparation method and application thereof

Through jet deposition technology and densification treatment, the particle size, distribution uniformity and oxygen content of high scandium-content aluminum scandium alloy targets are solved, and the aluminum scandium alloy target with fine particles, low oxygen content and uniform composition is realized, simplifying The process is reduced and the cost is improved, and the performance of microelectromechanical components is improved.

CN116117139BActive Publication Date: 2024-11-22HUNAN ORIENTAL SCANDIUM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310169272.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-11-22
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

In the prior art, when producing aluminum scandium alloy targets with high scandium content, Al3Sc particles are large, unevenly distributed, cracks, many hole defects, complex process, high oxygen content and high cost.

Method used

The spray deposition technology is used to quickly solidify the aluminum scandium alloy ingot and weld it layer by layer. Combined with densification and machining, a small, low oxygen content and uniform composition aluminum scandium alloy target is obtained.

Benefits of technology

Aluminum scandium alloy target with fine Al3Sc particles, low oxygen content, uniform composition and no cracks is realized, which simplifies the process flow, reduces production costs, is suitable for factory production, and improves the performance of microelectromechanical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116117139B_ABST
    Figure CN116117139B_ABST
Patent Text Reader

Abstract

The present invention provides an aluminum-scandium alloy target material and a preparation method and application thereof, and relates to the technical field of aluminum alloy target material processing, comprising the following steps: an aluminum-scandium alloy ingot is subjected to spray deposition to obtain an aluminum-scandium alloy target blank, and then subjected to densification treatment and machining to obtain an aluminum-scandium alloy target material. The present invention solves the technical problems of large Al3Sc particles, uneven distribution, and many cracks and pore defects when producing aluminum-scandium alloy targets with high scandium content by casting in the prior art, and also avoids the problems of complex process, high oxygen content and high price during powder metallurgy production, and achieves the technical effects of fine Al3Sc particles, low oxygen content, uniform composition and no cracks in the aluminum-scandium alloy target material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy target material processing, and in particular to an aluminum-scandium alloy target material and a preparation method and application thereof. Background Art

[0002] Aluminum-scandium alloy targets (AlSc) are used in the 3C industry as thin film materials for chips and can significantly improve the piezoelectric properties of electronic components, such as micro-electromechanical components (MEMS).

[0003] Aluminum-scandium alloy targets with scandium contents between 8 and 45 at% Sc (atomic ratio) are all used. The piezoelectric properties of aluminum-scandium alloy targets increase with the increase of scandium content, but also increase the difficulty of production. Common methods for making aluminum-scandium alloy targets include smelting casting and machining, which are simple processes. However, when the scandium content is >15 at% Sc, the casting method usually causes cracks, holes, and uneven composition in the ingot, making it impossible to produce high-quality targets. Common improvement methods include powder metallurgy, pressing and sintering, but there are problems of long process and high cost. At the same time, during the preparation and pressing process, the powder is in contact with air for a long time, which will lead to the problem of high oxygen content.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for preparing an aluminum-scandium alloy target material, which has a simple process and is easy to operate, and can prepare an aluminum-scandium alloy target material with fine Al3Sc particles, low oxygen content, uniform composition and no cracks.

[0006] The second object of the present invention is to provide an aluminum-scandium alloy target material having the advantages of fine Al3Sc particles, low oxygen content, uniform composition and no cracks.

[0007] The third object of the present invention is to provide an application of an aluminum-scandium alloy target material, which is beneficial to improving the performance of micro-electromechanical components and has outstanding application effects.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, a method for preparing an aluminum-scandium alloy target comprises the following steps:

[0010] The aluminum-scandium alloy ingot is spray-deposited to obtain an aluminum-scandium alloy target blank, which is then subjected to densification treatment and machining to obtain the aluminum-scandium alloy target material.

[0011] Furthermore, the spray deposition method comprises the following steps:

[0012] The aluminum-scandium alloy ingot is melted in a spray deposition furnace to obtain a melt, which is then injected into a ladle, and then spray-deposited on a collecting plate and cooled to obtain the aluminum-scandium alloy target blank;

[0013] Preferably, the vacuum degree of the spray deposition furnace is 3×10 -2 ~3×10 -3 MPa;

[0014] Preferably, the temperature of the melt is 1000-1500°C;

[0015] Preferably, the temperature of the leaking bag is 800-1000°C.

[0016] Furthermore, the diameter of the spray-deposited flow guide tube is 2 to 5 mm;

[0017] Preferably, the atomizing gas for the spray deposition comprises at least one of Ar and N2;

[0018] Preferably, the pressure of the atomizing gas is 0.5-2 MPa;

[0019] Preferably, the deposition distance of the spray deposition is 100-400 mm.

[0020] Furthermore, the rotation speed of the collecting plate is 50 to 100 rpm;

[0021] Preferably, the descending speed of the collecting plate is 10 to 500 mm / min;

[0022] Preferably, the collection tray comprises a collection tray with a cooling function;

[0023] Preferably, the cooling method includes cooling with cooling water;

[0024] Preferably, the water pressure of the cooling water is 1-2 MPa.

[0025] Furthermore, the method for preparing the aluminum-scandium alloy ingot comprises the following steps:

[0026] Mixing and smelting metal aluminum and metal scandium to obtain the aluminum-scandium alloy ingot;

[0027] Preferably, the smelting comprises vacuum smelting;

[0028] Preferably, the vacuum degree of the smelting is 3×10 -2 ~3×10 -3 MPa;

[0029] Preferably, the smelting temperature is 1000-1500° C., and the smelting time is 0.5-1 h.

[0030] Further, the densification treatment includes isostatic pressing;

[0031] Preferably, the temperature of the isostatic pressing treatment is 500-700°C;

[0032] Preferably, the pressure of the isostatic pressing treatment is 100-300 MPa, and the time of the isostatic pressing treatment is 3-5 hours.

[0033] Further, the machining includes wire cutting;

[0034] Preferably, the machining further includes the steps of flaw detection and welding.

[0035] In a second aspect, an aluminum-scandium alloy target is prepared by any of the preparation methods described above.

[0036] Furthermore, the scandium content of the aluminum-scandium alloy target is above 15at%;

[0037] Preferably, the oxygen content of the aluminum-scandium alloy target is 100 to 600 ppm;

[0038] Preferably, the size of Al3Sc particles in the aluminum-scandium alloy target is 25-80 μm.

[0039] A third aspect is an application of the aluminum-scandium alloy target described in any one of the above items in the preparation of micro-electromechanical components.

[0040] Compared with the prior art, the present invention has at least the following beneficial effects:

[0041] The preparation method of the aluminum-scandium alloy target provided by the present invention adopts the spray deposition technology. After the aluminum-scandium alloy is deposited, it can be quickly solidified and welded layer by layer. It is particularly suitable for the production of aluminum-scandium target materials of high-scandium alloy (20-45at% Sc). The alloy target material obtained thereby has the characteristics of fine Al3Sc particles, low oxygen content, uniform composition and no cracks, etc., which solves the technical problems of large Al3Sc particles, uneven distribution, many cracks and holes, complex process, high oxygen content and high cost in the production of aluminum-scandium alloy targets with high scandium content in the prior art. The preparation method provided by the present invention has a simple process, is easy to operate, and is suitable for factory production.

[0042] The aluminum-scandium alloy target material provided by the present invention has the advantages of fine Al3Sc particles, low oxygen content, uniform composition and no cracks.

[0043] The application of the aluminum-scandium alloy target material provided by the present invention is beneficial to improving the performance of micro-electromechanical components and has outstanding application effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0045] Figure 1 A flow chart of the preparation of an aluminum-scandium alloy target provided in Example 1 of the present invention;

[0046] Figure 2 Schematic diagram of the spray deposition of the aluminum-scandium alloy target provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0047] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] According to a first aspect of the present invention, there is provided a method for preparing an aluminum-scandium alloy target, comprising the following steps:

[0049] The aluminum-scandium alloy ingot is spray-deposited to obtain an aluminum-scandium alloy target blank, which is then subjected to densification treatment and machining to obtain an aluminum-scandium alloy target material.

[0050] The preparation method of the aluminum-scandium alloy target provided by the present invention adopts the spray deposition technology. After the aluminum-scandium alloy is deposited, it can be quickly solidified and welded layer by layer. It is particularly suitable for the production of aluminum-scandium target materials of high-scandium alloy (20-45at% Sc). The alloy target material obtained thereby has the characteristics of fine Al3Sc particles, low oxygen content, uniform composition and no cracks, etc., which solves the technical problems of large Al3Sc particles, uneven distribution, many cracks and holes, complex process, high oxygen content and high cost in the production of aluminum-scandium alloy targets with high scandium content in the prior art. The preparation method provided by the present invention has a simple process, is easy to operate, and is suitable for factory production.

[0051] In a preferred embodiment, the method of spray deposition of the present invention comprises the following steps:

[0052] The aluminum-scandium alloy ingot is melted in a spray deposition furnace to obtain a melt, which is then injected into a ladle, and then spray-deposited on a collecting plate and cooled to obtain an aluminum-scandium alloy target blank.

[0053] In a preferred embodiment, the temperature of the melt can be 1000-1500°C, and typical but non-limiting temperatures are, for example, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, and 1500°C; the temperature of the leaking bag can be 800-1000°C, and typical but non-limiting temperatures are, for example, 800°C, 820°C, 840°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, and 1000°C.

[0054] The preferred melt temperature and leak temperature in the present invention are more conducive to ensuring the fluidity of the melt, while ensuring that the melt will not have the problem of Al3Sc precipitation, and are more conducive to improving the preparation effect of the aluminum-scandium alloy target.

[0055] In a preferred embodiment, the diameter of the spray-deposited flow guide tube may be 2-5 mm, for example, 2 mm, 3 mm, 4 mm, 5 mm, but not limited thereto, which is more conducive to improving the conveying effect of the raw materials.

[0056] In a preferred embodiment, the vacuum degree of the spray deposition furnace can be 3×10 -2 ~3×10 -3 MPa, which is more conducive to eliminating the influence of oxygen and obtaining an aluminum-scandium alloy target with a low oxygen content.

[0057] In the present invention, the spray deposition process is carried out under high vacuum and protective atmosphere, which can ensure that the oxygen content of the aluminum-scandium alloy target is lower than 100-600 ppm and has high efficiency, which is incomparable to powder molding.

[0058] In the present invention, the process of spray deposition can be regarded as layer-by-layer solidification, which has the advantages of uniform heat distribution and metal shrinkage, so the product is crack-free, which is obviously unachievable for alloys with high scandium content prepared by melt casting.

[0059] In a preferred embodiment, the atomizing gas (protective atmosphere) for spray deposition includes but is not limited to at least one of Ar and N2. The atomizing gas must be of high purity and low oxygen content to avoid oxidation of the molten metal.

[0060] In a preferred embodiment, the pressure of the atomizing gas may be 0.5-2 MPa, and typical but non-limiting pressures are, for example, 0.5 MPa, 1 MPa, 1.5 MPa, and 2 MPa.

[0061] The atomizing gas pressure of the present invention is between 0.5 and 2 MPa, which is one of the key factors for controlling the synchronization of deposition rate and cooling rate. If the atomizing gas pressure is too high, the molten metal will not have time to solidify. If the atomizing gas pressure is too low, faults and holes will appear in the metal, and the efficiency will be low. The atomizing gas pressure of the present invention is only between 0.5 and 2 MPa to ensure rapid solidification of the metal, insufficient growth of Al3Sc particles and uniform distribution.

[0062] In a preferred embodiment, the deposition distance of the spray deposition may be 100-400 mm, and typical but non-limiting distances are, for example, 100 mm, 150 mm, 200 mm, 250 mm, 300 mm, 350 mm, and 400 mm.

[0063] In a preferred embodiment, the rotation speed of the collecting plate may be 50-100 rpm, and typical but non-limiting rotation speeds are, for example, 50 rpm, 60 rpm, 70 rpm, 80 rpm, 90 rpm, and 100 rpm.

[0064] The preferred deposition distance and collection plate rotation speed in the present invention can ensure that the metal is uniformly deposited on the collection plate, which is beneficial to improving the preparation effect of the aluminum-scandium alloy target.

[0065] In a preferred embodiment, the descending speed of the collecting plate can be 10 to 500 mm / min, and its typical but non-limiting descending speeds are, for example, 10 mm / min, 50 mm / min, 100 mm / min, 150 mm / min, 200 mm / min, 250 mm / min, 300 mm / min, 350 mm / min, 400 mm / min, 450 mm / min, and 500 mm / min.

[0066] In a preferred embodiment, the collecting tray includes a collecting tray with a cooling function, wherein the cooling method includes but is not limited to cooling with cooling water, which is beneficial to the rapid cooling of the spray deposition and is beneficial to improving the preparation effect of the aluminum-scandium alloy target blank.

[0067] In a preferred embodiment, the water pressure of the cooling water can be 1-2 MPa, and typical but non-limiting water pressures are, for example, 1 MPa, 1.2 MPa, 1.3 MPa, 1.4 MPa, 1.5 MPa, 1.6 MPa, 1.7 MPa, 1.8 MPa, 1.9 MPa, and 2 MPa.

[0068] The process parameters of the present invention, including the descending speed of the collecting plate and the water pressure of the cooling water, are all means for coordinating and adjusting the metal deposition speed. The various process parameters can cooperate with each other to obtain a high-quality alloy target blank after the deposition is completed, which is beneficial to improving the quality of the aluminum-scandium alloy target material.

[0069] In a preferred embodiment, the method for preparing the aluminum-scandium alloy ingot comprises the following steps:

[0070] Metallic aluminum and metallic scandium are mixed and smelted to obtain an aluminum-scandium alloy ingot.

[0071] In a preferred embodiment, the smelting temperature may be 1000-1500°C, and typical but non-limiting temperatures are, for example, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, and 1500°C.

[0072] In the present invention, a suspension furnace can be used for smelting, which can avoid crucible contamination caused by high-temperature and long-term alloying.

[0073] In the present invention, since the rare earth metal scandium is highly active and easily oxidized, the smelting method is preferably vacuum smelting, which can reduce the oxygen content of the aluminum-scandium alloy ingot.

[0074] In a preferred embodiment, the vacuum degree of melting can be 3×10 -2 ~3×10 -3 MPa, high vacuum can effectively reduce the oxygen content of the aluminum-scandium alloy ingot, otherwise the oxygen content will be too high and cannot be removed in subsequent processes.

[0075] In a preferred embodiment, the smelting time may be 0.5 to 1 h, and typical but non-limiting times are, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, and 1 h.

[0076] In the present invention, the composition after smelting and alloying is uniform, and then cast into a water-cooled copper mold for rapid cooling, which is beneficial to ensure the fine and uniform distribution of Al3Sc precipitated particles in the alloy, thereby obtaining a high-quality alloy ingot.

[0077] In a preferred embodiment, the densification treatment includes but is not limited to isostatic pressing. The alloy target blank obtained by spray deposition in the present invention will inevitably have fine defects, so it needs to be densified by isostatic pressing to ensure the high quality of the alloy target.

[0078] In a preferred embodiment, the temperature of the isostatic pressing treatment can be 500-700°C, and typical but non-limiting temperatures are, for example, 500°C, 550°C, 600°C, 650°C, and 700°C; the pressure of the isostatic pressing treatment can be 100-300MPa, and typical but non-limiting pressures are, for example, 100MPa, 150MPa, 200MPa, 250MPa, and 300MPa; the time of the isostatic pressing treatment can be 3-5h, and typical but non-limiting times are, for example, 3h, 3.5h, 4h, 4.5h, and 5h.

[0079] The process parameters of the isostatic pressing treatment of the present invention are more conducive to improving the densification treatment effect of the alloy target blank to ensure the high quality of the alloy target material.

[0080] In a preferred embodiment, the present invention further comprises the following steps after the densification process:

[0081] The alloy target blank after densification treatment is subjected to wire cutting and machining according to the preset required size and finish, and is subjected to flaw detection inspection to obtain a processed target;

[0082] The processed target is welded to the back plate of the substrate by vacuum diffusion welding to obtain an aluminum-scandium alloy target material.

[0083] In a preferred embodiment, the substrate includes but is not limited to 6063 aluminum.

[0084] According to a second aspect of the present invention, there is provided an aluminum-scandium alloy target prepared by any of the preparation methods described above.

[0085] In a preferred embodiment, the scandium content of the aluminum-scandium alloy target of the present invention is above 15 at %, preferably 20 to 45 at % Sc.

[0086] In a preferred embodiment, the oxygen content of the aluminum-scandium alloy target of the present invention is 100-600 ppm.

[0087] In a preferred embodiment, the size of Al3Sc particles in the aluminum-scandium alloy target of the present invention is 25-80 μm.

[0088] It can be seen that the aluminum-scandium alloy target provided by the present invention has the advantages of fine Al3Sc particles, low oxygen content, uniform composition and no cracks.

[0089] According to a third aspect of the present invention, there is provided a use of the aluminum-scandium alloy target material described in any one of the above items in the preparation of micro-electromechanical components.

[0090] The application of the aluminum-scandium alloy target material provided by the present invention is beneficial to improving the performance of micro-electromechanical components and has outstanding application effects.

[0091] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0092] Example 1

[0093] A method for preparing an aluminum-scandium alloy target, see Figure 1 , including the following steps:

[0094] S1: Composition requirements: Aluminum-scandium alloy target 20at%Sc;

[0095] High-purity aluminum and scandium are prepared according to the composition requirements, placed in a vacuum magnetic levitation melting furnace, and heated and melted under vacuum. The vacuum degree is 5×10 -2 MPa, temperature 1300℃, keep warm for 0.5h, then cast into a water-cooled copper mold to obtain an aluminum-scandium alloy ingot;

[0096] S2: spray deposition, see Figure 2 The aluminum-scandium alloy ingot is placed in a vacuum spray deposition furnace, vacuumed and heated to melt, with a vacuum degree of 3×10 -2 MPa, molten metal temperature 1300℃, poured into the ladle, the ladle is heated to 800℃, the guide tube diameter Ar was used for atomization (pressure 0.5 MPa), the deposition distance was 150 mm, and the sample was deposited on a collector with cooling (v1 speed 50 rpm, v2 descending speed 10 mm / min, cooling water cooling, water pressure 1.5 MPa), to obtain an aluminum-scandium alloy target blank (wherein the Al3Sc particle size was 45 μm and the oxygen content was 450 ppm);

[0097] S3: The aluminum-scandium alloy target blank is placed in a hot isostatic pressing furnace and subjected to densification treatment at 700° C. and 200 MPa for 5 h to obtain a densified target blank;

[0098] S4: The densified target blank is subjected to wire cutting, machining and flaw detection according to preset size requirements and finish to obtain a processed target;

[0099] S5: The processed target is welded to a back plate whose substrate is 6063 aluminum material by vacuum diffusion welding to obtain an aluminum-scandium alloy target.

[0100] Example 2

[0101] A method for preparing an aluminum-scandium alloy target comprises the following steps:

[0102] S1: Composition requirements: Aluminum-scandium alloy target 30at%Sc;

[0103] High-purity aluminum and scandium are prepared according to the composition requirements, placed in a vacuum magnetic levitation melting furnace, and heated and melted under vacuum. The vacuum degree is 3×10 -3 MPa, temperature 1500℃, keep warm for 1h, then cast into a water-cooled copper mold to obtain an aluminum-scandium alloy ingot;

[0104] S2: Spray deposition: The aluminum-scandium alloy ingot is placed in a vacuum spray deposition furnace, vacuumed, heated and melted, with a vacuum degree of 3×10 -3 MPa, molten metal temperature 1500℃, poured into the ladle, the ladle is heated to 1000℃, the guide tube diameter Ar was used for atomization (pressure 1.2 MPa), the deposition distance was 200 mm, and the particles were deposited on a collector with cooling (v1 speed 75 rpm, v2 descending speed 50 mm / min, cooling water cooling, water pressure 2 MPa), to obtain an aluminum-scandium alloy target blank (wherein the Al3Sc particle size was 65 μm and the oxygen content was 550 ppm);

[0105] S3: the aluminum-scandium alloy target blank is placed in a hot isostatic pressing furnace and subjected to densification treatment at 660° C. and 100 MPa for 3 h to obtain a densified target blank;

[0106] S4: The densified target blank is subjected to wire cutting, machining and flaw detection according to preset size requirements and finish to obtain a processed target;

[0107] S5: The processed target is welded to a back plate whose substrate is 6063 aluminum material by vacuum diffusion welding to obtain an aluminum-scandium alloy target.

[0108] Example 3

[0109] A method for preparing an aluminum-scandium alloy target comprises the following steps:

[0110] S1: Composition requirements: Aluminum-scandium alloy target 15at%Sc;

[0111] High-purity aluminum and scandium are prepared according to the composition requirements, placed in a vacuum magnetic levitation melting furnace, and heated and melted under vacuum. The vacuum degree is 3×10 -3 MPa, temperature 1200℃, keep warm for 1.5h, then cast into a water-cooled copper mold to obtain an aluminum-scandium alloy ingot;

[0112] S2: Spray deposition: The aluminum-scandium alloy ingot is placed in a vacuum spray deposition furnace, vacuumed, heated and melted, with a vacuum degree of 3×10 -2 MPa, molten metal temperature 1200℃, poured into the ladle, the ladle is heated to 900℃, the guide tube diameter Ar was used for atomization (pressure 1.5 MPa), the deposition distance was 350 mm, and the sample was deposited on a collector with cooling (v1 speed 60 rpm, v2 descending speed 15 mm / min, cooling water cooling, water pressure 1.2 MPa), to obtain an aluminum-scandium alloy target blank (wherein the Al3Sc particle size was 25 μm and the oxygen content was 150 ppm);

[0113] S3: the aluminum-scandium alloy target blank is placed in a hot isostatic pressing furnace and subjected to densification treatment at 660° C. and 150 MPa for 4 h to obtain a densified target blank;

[0114] S4: The densified target blank is subjected to wire cutting, machining and flaw detection according to preset size requirements and finish to obtain a processed target;

[0115] S5: The processed target is welded to a back plate whose substrate is 6063 aluminum material by vacuum diffusion welding to obtain an aluminum-scandium alloy target.

[0116] The preparation method of the present invention solves the technical problems of the prior art in producing aluminum-scandium alloy targets with high scandium content by casting, such as large Al3Sc particles, uneven distribution, and many cracks and pore defects. It also avoids the problems of complex process, high oxygen content and high price in powder metallurgy production, and achieves the technical effect that the Al3Sc particles of the aluminum-scandium alloy targets are small, low in oxygen content, uniform in composition and free of cracks.

[0117] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an aluminum-scandium alloy target, characterized in that: The following steps are involved: The aluminum-scandium alloy ingot is subjected to spray deposition to obtain an aluminum-scandium alloy target blank, which is then subjected to densification treatment and machining to obtain the aluminum-scandium alloy target material; The method of spray deposition comprises the following steps: The aluminum-scandium alloy ingot is melted in a spray deposition furnace to obtain a melt, which is then injected into a ladle, and then spray-deposited on a collecting plate and cooled to obtain the aluminum-scandium alloy target blank; The vacuum degree of the spray deposition furnace is 3×10 -2 ~3×10 -3 MPa; The temperature of the melt is 1000-1500°C; The temperature of the leaking bag is 800-1000°C; The diameter of the spray-deposited flow guide tube is 2 to 5 mm; The atomizing gas for the spray deposition includes at least one of Ar and N2; The pressure of the atomizing gas is 0.5~2 MPa; The deposition distance of the spray deposition is 100-400 mm; The rotation speed of the collecting plate is 50-100 rpm; The descending speed of the collecting plate is 10-500 mm / min; The collecting tray comprises a collecting tray with a cooling function; The cooling method includes cooling with cooling water; The water pressure of the cooling water is 1~2 MPa; The method for preparing the aluminum-scandium alloy ingot comprises the following steps: Mixing and smelting metal aluminum and metal scandium to obtain the aluminum-scandium alloy ingot; The smelting includes vacuum smelting; The vacuum degree of the smelting is 3×10 -2 ~3×10 -3 MPa; The smelting temperature is 1000-1500°C, and the smelting time is 0.5-1 h; The densification treatment includes isostatic pressing; The temperature of the isostatic pressing treatment is 500-700°C; The pressure of the isostatic pressing treatment is 100-300 MPa, and the time of the isostatic pressing treatment is 3-5 h; The scandium content of the aluminum-scandium alloy target is above 15 at %; The oxygen content of the aluminum-scandium alloy target is 100-600 ppm; The size of Al3Sc particles in the aluminum-scandium alloy target is 25-80 μm.

2. The preparation method according to claim 1, characterized in that: The machining includes wire cutting; The machining process is followed by flaw detection and welding.

3. Use of the aluminum-scandium alloy target prepared by the preparation method according to claim 1 or 2 in the preparation of micro-electromechanical components.