A steel slag concrete 3D printing material and its preparation method and use
By using steel slag as the main raw material, the steel slag concrete 3D printing material is prepared, which solves the performance and environmental protection problems of 3D printing materials, achieves the effects of high strength, low cost and resource regeneration, and overcomes the shortcomings of traditional materials.
Patent Information
- Application Number
- CN202211531858.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-01
AI Technical Summary
The existing 3D printed concrete materials have shortcomings in performance and environmental protection, making it difficult to take into account appropriate fluidity and strength, and at the same time, they fail to effectively utilize industrial solid waste, resulting in waste of resources and environmental pollution.
Steel slag is used as the main raw material to prepare 3D printing materials for steel slag concrete through specific formulas and processing processes, including fine-grained steel slag powder, steel slag aggregate, special fine sand of steel slag, cement, early strength agent, thickener and superplasticizer. Combining processes such as crushing, screening and magnetic separation, a suitable 3D printing ink is formed.
The strength indicators of 3D printing materials have been improved, natural resources have been saved, the use of cement and fly ash has been reduced, the recycling of resources has been realized, production costs have been reduced, and the stability and environmental performance of the materials have been improved.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to concrete building materials, and in particular to a steel slag concrete 3D printing material and a preparation method and application thereof. Background Art
[0002] 3D printing is a new additive manufacturing technology that is booming. It started abroad and has developed rapidly in China in recent years. 3D printing technology can be applied to prefabricated buildings, which have many advantages over traditional construction.
[0003] Prefabricated buildings have higher quality, and all of their components can be processed into integral wall panels, beams, columns and floor slabs as needed, and water pipes, wires, windows, etc. can be pre-buried in the structural building. Fixed molds promote the formalization, scientificization and integration of the production process, which promotes a significant improvement in building quality. Since all of its components are prefabricated in the factory workshop and only need to be assembled on site, it also effectively reduces labor costs and saves manpower and material resources. The use of 3D printing technology to produce building components is more accurate and more efficient. At the same time, it can also make full use of various industrial solid wastes, which is economical and environmentally friendly, reduces the production of construction waste, and saves energy and emissions.
[0004] Since my country's 3D printing technology started late, it is not mature enough compared with developed countries such as the United States and Germany. In particular, some related standards are not yet perfect, and there is still a lot of room for optimization of raw material formulas and process flows. In the 3D printing process, the performance of the materials used for printing is extremely important. In order to make the concrete for 3D printing have appropriate fluidity and ensure that its strength is not greatly affected, and taking into account the green and low-carbon development concept and economic benefits, the formula of 3D printing concrete needs to continue to be studied. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a steel slag concrete 3D printing material and a preparation method and use thereof, so as to solve the problems in the prior art.
[0006] To achieve the above objectives and other related objectives, the present invention is obtained by including the following technical solutions.
[0007] The present invention provides a steel slag concrete 3D printing material, comprising the following raw material components in parts by weight:
[0008]
[0009]
[0010] Preferably, the cement content may be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20.
[0011] Preferably, the content of the ground steel slag powder may be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20. More preferably, the content of the ground steel slag powder is 10 to 20 parts by weight.
[0012] Preferably, the content of the steel slag aggregate may be 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 or 35. More preferably, the content of the steel slag aggregate is 25-30.
[0013] Preferably, the content of the steel slag special fine sand may be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20. More preferably, the content of the steel slag special fine sand is 15-20.
[0014] Preferably, the water content may be 10, 11, 12, 13, 14 or 15.
[0015] Preferably, the particle size of the steel slag aggregate is 3-5 mm. It is obtained by crushing and screening the steel slag raw material. The steel slag raw material is electric furnace steel slag or converter steel slag produced by Baosteel Co., Ltd. steelmaking.
[0016] Preferably, the slag aggregate has a screening content of ≥90% within the range of 3 to 5 mm using a square hole sieve.
[0017] Preferably, the steel slag concrete 3D printing material further includes 2 to 5 parts by weight of an early strength agent.
[0018] Preferably, the steel slag concrete 3D printing material further includes 0.01 to 0.05 parts by weight of a thickener.
[0019] Preferably, the steel slag concrete 3D printing material further includes 0.1 to 0.5 parts by weight of a superplasticizer.
[0020] Preferably, the porosity of the steel slag aggregate is ≤2%.
[0021] Preferably, the MFe of the steel slag aggregate is ≤1%.
[0022] Preferably, the free calcium oxide content of the steel slag aggregate is ≤3%.
[0023] Preferably, the cement is P.O42.5 ordinary Portland cement.
[0024] The ground steel slag powder in this application refers to the steel slag produced by converter and electric furnace steelmaking, which is prepared into a powder product with a certain fineness through drying, crushing, sorting, magnetic separation and grinding.
[0025] Preferably, the 45 μm screen residue rate of the ground steel slag powder is less than 2%. The test method is GB / T1345.
[0026] Preferably, the MFe content of the ground steel slag powder is ≤ 1%, and the test method is YB / T 140.
[0027] Preferably, the free calcium oxide content in the ground steel slag powder is ≤3%. Free calcium oxide is f.CaO, and its test method is YB / T 140.
[0028] Preferably, the specific surface area of the ground steel slag powder is ≥360m 2 / kg. The test method is GB / T8074.
[0029] Preferably, the particle size of the steel slag special fine sand ranges from 0 to 3 mm.
[0030] Preferably, the screening content of the steel slag special fine sand in the particle size range of 0 to 3 mm through a square hole sieve is ≥90%.
[0031] Preferably, the porosity of the steel slag special fine sand is ≤2%.
[0032] Preferably, the MFe in the steel slag special fine sand is ≤1%.
[0033] Preferably, the free calcium oxide content in the steel slag special fine sand is ≤3%.
[0034] Preferably, the regenerated sand is construction regenerated sand, and the particle size of the regenerated sand is 0.25-0.5 mm.
[0035] Preferably, the early strength agent does not contain chlorine and has a moisture content of ≤5%.
[0036] Preferably, the thickener is a mixture of polyacrylamide and cellulose ether. More preferably, the mass ratio of the polyacrylamide to the cellulose ether is 1:(0.5-2).
[0037] Preferably, the superplasticizer is a polycarboxylic acid water reducer. The density of the superplasticizer is 1.02-1.08 g / cm 3 , pH is 6-8.
[0038] The present invention also discloses a method for preparing the steel slag concrete 3D printing material as described above, which comprises mixing the raw material components.
[0039] The present invention also provides a use of the steel slag concrete 3D printing material as described above as a 3D printing ink for construction.
[0040] The beneficial effects of the above technical solution of the present invention are:
[0041] 1) All strength indicators of the processed 3D printing materials are above the standard requirements of architectural 3D printing inks, and the performance is good;
[0042] 2) Use steel slag fine sand and recycled sand to replace the common natural river sand in aggregates, saving natural resources;
[0043] 3) Reduce the amount of cement and fly ash added, reduce costs and improve stability;
[0044] 4) Take advantage of steel slag solid waste, overcome the defects of the original materials, prepare 3D printed concrete products that meet performance standards, turn waste into treasure and achieve resource recycling. DETAILED DESCRIPTION
[0045] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0046] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0047] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between the steps explicitly mentioned, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. The change or adjustment of their relative relationship shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0048] The specific formulations of Examples 1 to 3 in this application are shown in Table 1 below. The contents in the table are in parts by weight.
[0049] The components in each embodiment and comparative example were mixed uniformly.
[0050] Specifically, the particle size of the steel slag aggregate in the embodiment is 3-5 mm. It is obtained by crushing and screening the steel slag raw material. The steel slag raw material is electric furnace steel slag or converter steel slag produced by Baosteel Co., Ltd.; the screening content of the steel slag aggregate within 3-5 mm using a square hole sieve is ≥90%; the porosity of the steel slag aggregate is ≤2%; the MFe of the steel slag aggregate is ≤1%; the free calcium oxide content of the steel slag aggregate is ≤3%.
[0051] Specifically, the cement is P.O42.5 ordinary Portland cement.
[0052] The ground steel slag powder in the embodiment of the present application refers to the steel slag produced by converter and electric furnace steelmaking, which is dried, crushed, sorted, magnetically separated and ground into a powder product of a certain fineness. The 45μm sieving rate of the ground steel slag powder in the embodiment is less than 2%. The test method is GB / T1345; the MFe content of the ground steel slag powder is ≤1%. The test method is YB / T 140; the free calcium oxide content in the ground steel slag powder is ≤3%. Free calcium oxide is f.CaO, and the test method is YB / T 140; the specific surface area of the ground steel slag powder is ≥360m 2 / kg. The test method is GB / T8074.
[0053] Specifically, the particle size range of the steel slag special fine sand in the embodiment is 0-3 mm; the screening content of the steel slag special fine sand in the particle size range of 0-3 mm by the square hole sieve is ≥90%, the porosity of the steel slag special fine sand is ≤2%, the MFe in the steel slag special fine sand is ≤1%; the free calcium oxide content in the steel slag special fine sand is ≤3%.
[0054] Specifically, the regenerated sand in the embodiment is construction regenerated sand, and the particle size of the regenerated sand is 0.25-0.5 mm.
[0055] Specifically, the early strength agent described in the embodiment does not contain chlorine and has a moisture content of ≤5%; it is specifically a chemically modified composite concrete early strength agent produced by Wuhan Jiyesheng Chemical Co., Ltd.
[0056] Specifically, the thickener is a mixture of polyacrylamide and cellulose ether.
[0057] Specifically, the superplasticizer is a polycarboxylate water reducer, and the density of the superplasticizer is 1.02-1.08 g / cm 3 , pH is 6 to 8. It is a white to light yellow viscous liquid.
[0058] Table 2 and Table 3 are the formulas and test results in the comparative examples.
[0059] Table 1
[0060]
[0061]
[0062] Table 2
[0063]
[0064]
[0065] Table 3
[0066]
[0067]
[0068] From the test results of Examples 1-3, it can be seen that the formed steel slag concrete 3D printing material can reach the performance index of I40 in Q31 / 0116000628C005-2018 "3D Printing Ink for Construction". The compressive strength, splitting tensile strength, axial compressive strength and flexural strength test methods in this application refer to GB / T 50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete" and meet the requirements of this standard; the frost resistance, shrinkage and early crack resistance test methods refer to GB / T50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete" and meet the requirements of this standard, so it is feasible.
[0069] Under the premise of achieving the same performance, the embodiment can add 10%-15% less cement than the comparative examples 1-2, and the economic benefit is better.
[0070] The waste utilization rate of the embodiment can reach 50%-80%, and compared with comparative examples 1-2, 500-800 kg of natural resources can be saved per ton.
[0071] Compared with Comparative Examples 1-2, Examples 1-3 have advantages in mechanical properties such as compressive strength, splitting tensile strength and flexural strength, are basically the same in frost resistance, and have certain advantages in early crack resistance.
[0072] Example 4 is a comparative example of Example 1. The difference between Example 4 and Example 1 is that no early strength agent is used. Other aspects are the same as Example 1. Without the early strength agent, the mechanical properties are reduced, but the antifreeze performance is not greatly affected.
[0073] Example 5 is a comparative example of Example 1. The difference between Example 5 and Example 1 is that polyacrylamide is not used. The other aspects are the same as Example 1. Without the addition of polyacrylamide, the mechanical properties are reduced, but the antifreeze performance is not greatly affected.
[0074] Example 6 is a comparative example of Example 1. The difference between Example 6 and Example 1 is that cellulose ether is not used. The other aspects are the same as Example 1. Without the addition of cellulose ether, the mechanical properties are reduced, and the reduction in crack resistance is more obvious.
[0075] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A steel slag concrete 3D printing material, characterized in that: The steel slag concrete 3D printing material includes the following raw material components in parts by weight: The steel slag aggregate has a screening content of ≥90% in the range of 3-5mm using a square hole sieve; the screening rate of the ground steel slag powder of 45μm is less than 2%; the screening content of the steel slag special fine sand in the range of 0-3mm using a square hole sieve is ≥90%; The steel slag concrete 3D printing material also includes 2 to 5 parts by weight of an early strength agent; The steel slag concrete 3D printing material also includes 0.01 to 0.05 parts by weight of a thickener; The steel slag concrete 3D printing material also includes 0.05 to 0.5 parts by weight of a superplasticizer.
2. The steel slag concrete 3D printing material according to claim 1, characterized in that: The porosity of the steel slag aggregate is ≤2%; and / or, the MFe of the steel slag aggregate is ≤1%; and / or, the free calcium oxide content of the steel slag aggregate is ≤3%.
3. The steel slag concrete 3D printing material according to claim 1, characterized in that: The cement is P.O42.5 ordinary Portland cement.
4. The steel slag concrete 3D printing material according to claim 1, characterized in that: The MFe content of the ground steel slag powder is ≤1%; and / or the free calcium oxide content of the ground steel slag powder is ≤3%; and / or the specific surface area of the ground steel slag powder is ≥360m 2 / kg.
5. The steel slag concrete 3D printing material according to claim 1, characterized in that: The porosity of the steel slag special fine sand is ≤2%; and / or, the MFe in the steel slag special fine sand is ≤1%; and / or, the free calcium oxide content in the steel slag special fine sand is ≤3%; and / or, the regenerated sand is construction regenerated sand, and the particle size of the regenerated sand is 0.25-0.5mm.
6. The steel slag concrete 3D printing material according to claim 1, characterized in that: The early strength agent does not contain chlorine and has a water content of ≤5%; and / or the thickener is a mixture of polyacrylamide and cellulose ether.
7. The steel slag concrete 3D printing material according to claim 6, characterized in that: The mass ratio of the polyacrylamide to the cellulose ether is 1:(0.5-2).
8. A method for preparing the steel slag concrete 3D printing material as claimed in any one of claims 1 to 7, comprising mixing the raw material components.
9. Use of the steel slag concrete 3D printing material as claimed in any one of claims 1 to 7 as 3D printing ink for construction.
Citation Information
Cited By
Preparation method of 3D printing balancing weight shell
CN117103414A