Ultra-low density and high strength water-control fracturing proppant and preparation method thereof

Through the combination and process of fly ash and other materials, ultra-low-density and high-strength water-control fracturing proppant is prepared, which solves the problems of compressive strength and water locking effect in deep well fracturing, and achieves efficient oil-water separation and well Increased output.

CN116120039BActive Publication Date: 2024-10-15SHAANXI YANCHANG PETROLEUM GRP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202310156172.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-23
Publication Date
2024-10-15
Estimated Expiration
2043-02-23

AI Technical Summary

Technical Problem

Existing fracturing proppant is difficult to meet the compressive strength and low density requirements in deep or ultra-deep wells, and traditional processes consume high energy and cost, and suffer from water locking effects and oil-water separation problems.

Method used

Fly ash is used as the main component, combined with binders, reinforcing agents and water-reducing agents. After pelletizing and sintering, an activator is added to form a hydrophobic layer to prepare an ultra-low-density and high-strength water-control fracturing proppant.

Benefits of technology

The proppant achieves small size, high compressive strength and good acid dissolution resistance, reduces water flow resistance, improves oil mobility and well production, reduces formation water production, and reduces construction difficulty and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses an ultra-low density high-strength water-controlled fracturing proppant, wherein the raw materials of the proppant include a main component and an activator, wherein the mass ratio of the main component to the activator is 100:(10-15); the main component is calculated according to 100 parts by weight, and is composed of the following raw materials in parts by weight: 91-95 parts of fly ash, 1-4 parts of a binder, 2-5 parts of a reinforcing agent, and 0.1-0.5 parts of a water reducer; the activator is a mixture of hexamethylenetetramine and bisphenol A resin. At the same time, the preparation method of the proppant is also disclosed. The proppant provided by the present invention has small volume, high compressive strength, good acid-resistant dissolution rate, and a contact angle of a hydrophobic and oleophilic layer greater than 110° is formed to reduce the flow resistance of oil and increase the flow resistance of water, thereby increasing the single well production, reducing the formation water generation while maintaining the formation energy, effectively reducing the construction difficulty and cost, and increasing the economic benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum proppants, and in particular relates to an ultra-low density and high-strength water-control fracturing proppant and a preparation method thereof. Background Art

[0002] my country's coal resources are mainly used for thermal power generation, and coal-fired power plants generate a large amount of fly ash. Fly ash is the main solid waste discharged by coal-fired power plants and power plants that utilize coal gangue and coal slime. Only a small part of it is used, and most of it is stored. The main oxide components of fly ash in my country's thermal power plants are: SiO2, Al2O3, FeO, Fe2O3, CaO, TiO2, etc.

[0003] The comprehensive utilization of fly ash in my country has gone through three stages: "storage first" - "combination of storage and use" - "use first". At present, the main ways of comprehensive utilization of fly ash include production of cement, concrete and other building materials, construction engineering, soil improvement, backfilling, production of bio-compound fertilizer, extraction of materials for high-value utilization, etc., involving multiple fields such as building materials, construction, chemical industry and agriculture, and a number of professional fly ash comprehensive utilization enterprises have emerged.

[0004] Hydraulic fracturing is an important technical means to increase the production of oil and gas wells. Whether it is conventional low-permeability and ultra-low-permeability oil and gas reservoirs, or shale and tight sandstone reservoirs of unconventional oil and gas reservoirs, hydraulic fracturing plays a key role in increasing production, especially in unconventional reservoirs. Without hydraulic fracturing, it is difficult to extract the oil and gas underground. During the fracturing construction process, proppant is mixed into the fracturing fluid and injected into deep rock cracks by high pressure to support the rock formation, forming one or more cracks with certain geometric dimensions in the formation. The length of the crack is generally from tens of meters to hundreds of meters, the height is from several meters to tens of meters, and the width is several millimeters. After the fracturing is completed, the fracturing fluid breaks the gel and flows back to the ground. The proppant remains in the crack, plays the role of supporting the crack, and keeps the crack in an open state. The pores between the proppant particles provide a circulation channel for the formation oil, gas and water, thereby achieving the effect of fracturing to increase production.

[0005] With the continuous expansion of the development scale, the difficulty of reservoir development is also increasing. The continuous decline in oil well production and the increase in water content have become a problem that needs to be solved urgently. Fracturing proppant is an essential supporting material required by hydraulic fracturing technology during oil and gas production. It is one of the key factors for the effect of increasing production. Different types of proppants are selected according to the formation characteristics and depth characteristics of the fracturing area. During the fracturing transformation process, the cracks are easy to extend to the water layer, and the water invasion phenomenon is serious after fracturing, causing some well layers to be flooded prematurely, leading to formation energy exhaustion, greatly reducing the single well production and final recovery rate. The reservoir generally presents water-wet characteristics. When crude oil flows through conventional proppants with hydrophilic surfaces, it forms dispersed oil droplets due to the Jamin effect, making it more difficult for crude oil to pass through the pore throat. Traditional proppants mainly include natural sand, resin-coated sand, and ceramsite. They are non-selective proppants. They need to withstand large impact forces and closing stresses during use. Unfavorable factors such as backflow, embedding, dissolution, and crushing may occur. The propped fractures have too high water conductivity, which aggravates the water lock effect. Therefore, seeking a proppant with high compressive strength, low density, good sphericity, high conductivity, and increased water flow resistance, thereby reducing water output has always been one of the goals pursued in this field.

[0006] For example, Chinese patent CN115141032A discloses a low-density fly ash fracturing proppant and a preparation method thereof, which comprises fly ash, adhesive, flux, reinforcing agent, water reducing agent, mixing, shaping, drying, sintering at 1200°C, cooling, screening, and a crushing rate of about 7% at 52MPa. The compressive strength is low and cannot meet the demand for proppant for deep well or ultra-deep well fracturing; Chinese patent CN103805160A discloses a preparation method for a high-doped fly ash ceramsite proppant, which comprises bauxite, fly ash, calcite powder, talc powder, titanium dioxide, light refractory clay and barite powder, ball milling, granulation, drying, screening. , sintering, and the sintering temperature is 1350-1500°C, which consumes a lot of energy; Chinese patent CN103205248A discloses a method for preparing an oil fracturing proppant with fly ash and waste ceramics as main materials, supplemented by potassium feldspar powder and manganese ore powder, but the amount of fly ash added to the main material is too small, which affects the performance of the proppant; Chinese patent CN104479665A discloses an oil fracturing proppant with nickel-iron slag as raw material. This solution solves the resource utilization of nickel-iron slag to a certain extent, but the treatment method of nickel-iron slag in this solution is the same as the general method in the prior art, that is, the nickel-iron slag is ball-milled into powder and then granulated for use. The treatment method of granulating and sintering nickel-iron slag after grinding leads to high process energy consumption, which is not conducive to energy conservation and environmental protection, has high cost, and is not in line with the industrial reuse direction of nickel-iron slag solid waste resources; Chinese patent document CN103131406A discloses a super hydrophobic proppant and a preparation method, which uses a silane coupling agent, a mixing resin, a plasticizer, an amine curing agent and other raw materials to react with a proppant aggregate, and obtains an oleophilic and hydrophobic coated proppant through mechanical stirring. This modification method has many operating steps, many types of raw materials, and strict requirements on the selection of proppants. It is not suitable for all types of proppants and has a small scope of application. It not only increases the complexity of the process, but also increases the cost of proppant modification. Summary of the invention

[0007] In view of the defects of the prior art, the object of the present invention is to provide an ultra-low density and high-strength water-control fracturing proppant and a preparation method thereof, wherein the proppant has the characteristics of small volume, high compressive strength and good acid dissolution resistance.

[0008] An ultra-low density and high-strength water-control fracturing proppant, wherein the raw materials of the proppant include a main component and an activator, wherein the mass ratio of the main component to the activator is 100:(10-15); the main component is composed of the following raw materials in parts by weight based on 100 parts by weight: 91-95 parts of fly ash, 1-4 parts of a binder, 2-5 parts of a reinforcing agent, and 0.1-0.5 parts of a water reducer; and the activator is a mixture of hexamethylenetetramine and bisphenol A resin.

[0009] Preferably, the binder is any one or any combination of kaolin, clay, carboxymethyl cellulose, and liquid epoxy resin. The addition of the binder helps to stabilize the proppant.

[0010] Preferably, the reinforcing agent is any one or any combination of nickel-iron slag, naphthenic crude oil, and manganese oxide.

[0011] Preferably, the water reducer is a polycarboxylate water reducer.

[0012] The method for preparing the ultra-low density and high-strength water-control fracturing proppant comprises the following steps:

[0013] (1) Material preparation: prepare the main components, crush and grind the fly ash, pass it through a 200-mesh sieve, and dry it;

[0014] (2) Balling: Fly ash, binder, reinforcing agent and water reducing agent are added into a balling machine for balling at a temperature of 55-65°C. Water is continuously sprayed during the balling process to obtain proppant spheres.

[0015] (3) Sintering: Sintering the proppant spheres obtained in step (2) and then cooling them to room temperature;

[0016] (4) Activation: The proppant sintered and formed in step (3) is added into a pelletizing machine, and an activator is continuously added during the rolling process of the pelletizing machine to obtain an ultra-low density and high-strength water-controlling fracturing proppant.

[0017] Preferably, the drying condition in step (1) is drying at 105±2°C for 5-6h.

[0018] Preferably, the total amount of water sprayed in step (2) is 10-15% of the total amount of the main components.

[0019] Preferably, the particle size of the proppant spheres in step (2) is 0.5-0.8 mm.

[0020] Preferably, the sintering molding is specifically as follows: first, the temperature is increased to 600°C at 20-50°C / min, then the temperature is increased to 900°C at 30-60°C / min, and finally the temperature is increased to 1200°C at 5°C / min, and kept at this temperature for 2 hours.

[0021] The proppant provided by the present invention uses fly ash, an industrial solid waste, as a raw material, and selects particles with a particle size suitable for oil fracturing proppant produced during the fly ash crushing process. By adding a binder, a reinforcing agent, and a water reducing agent, the mixed combined raw materials are directly pelletized in a pelletizing machine to reach the required particle size range standard, and then enter sintering molding, and then the surface is activated and hydrophobic treatment is performed to finally obtain a finished product.

[0022] In the present invention, after the high temperature reaction, the reinforcing agent helps to generate needle-shaped alumina and rod-shaped grains that cross each other, and the water sprayed in the preparation process fills between each grain, so that the proppant obtains suitable strength and toughness. The addition of a water reducer can reduce the amount of water, reduce the energy consumption of drying, and at the same time improve the bonding inside the proppant green body, and improve the calcination strength. The addition of an activator can form a super hydrophobic layer on the surface of the proppant through a nucleophilic addition reaction.

[0023] Advantages of the present invention:

[0024] (1) The proppant provided by the present invention has a small volume, high compressive strength, good acid dissolution resistance, and can reduce the flow resistance of oil and increase the flow resistance of water by forming a hydrophobic and oleophilic layer with a contact angle greater than 110°, thereby increasing the single well production, reducing the generation of formation water and maintaining the formation energy, effectively reducing the construction difficulty and cost, and increasing the economic benefits;

[0025] (2) The proppant provided by the present invention provides an effective way to utilize fly ash with high added value, which is helpful for environmental protection and resource utilization of solid waste. DETAILED DESCRIPTION

[0026] Example 1

[0027] 1. An ultra-low density and high-strength water-control fracturing proppant, the raw materials include a main component and an activator, the main component is composed of fly ash, a binder, a reinforcing agent and a water reducer, and the weight parts of each raw material are as follows: 94 parts of fly ash, 3 parts of binder, 2.5 parts of reinforcing agent, 0.5 parts of polycarboxylic acid water reducer, 15 parts of activator,

[0028] Wherein, the binder is a mixture of carboxymethyl cellulose and liquid epoxy resin in a mass ratio of 0.5:2.5;

[0029] The enhancer is a mixture of naphthenic crude oil and manganese oxide in a mass ratio of 1.5:1;

[0030] The activator is a mixture of hexamethylenetetramine and bisphenol A resin in a mass ratio of 8:7.

[0031] 2. The method for preparing the ultra-low density and high strength water control fracturing proppant comprises the following steps:

[0032] (1) Material preparation: Prepare the main components, crush and grind the fly ash, pass it through a 200-mesh sieve, and dry it at 105±2℃ for 5h;

[0033] (2) Balling: Fly ash, binder, reinforcing agent and water reducing agent are added into a balling machine for balling at a temperature of 60°C. Water is sprayed continuously during the balling process, and the total amount of water sprayed is 15% of the total amount of the main components to obtain proppant spheres with a particle size of 0.5-0.8 mm.

[0034] (3) Sintering: Sinter the proppant spheres obtained in step (2) by first heating to 600°C at 20°C / min, then heating to 900°C at 30°C / min, and finally heating to 1200°C at 5°C / min, keeping the temperature for 2 h, and then cooling to room temperature;

[0035] (4) Activation: The proppant sintered and formed in step (3) is added into a pelletizing machine, and an activator is continuously added during the rolling process of the pelletizing machine to obtain an ultra-low density and high-strength water-controlling fracturing proppant.

[0036] Example 2

[0037] 1. An ultra-low density and high-strength water-control fracturing proppant, the raw materials include a main component and an activator, the main component is composed of fly ash, a binder, a reinforcing agent and a water reducer, and the weight parts of each raw material are as follows: 93 parts of fly ash, 4 parts of binder, 2.7 parts of reinforcing agent, 0.3 parts of polycarboxylic acid water reducer, 10 parts of activator,

[0038] Wherein, the binder is a mixture of carboxymethyl cellulose and liquid epoxy resin in a mass ratio of 1.5:2.5;

[0039] The enhancer is a mixture of naphthenic crude oil and manganese oxide in a mass ratio of 1.2:1.5;

[0040] The activator is a mixture of hexamethylenetetramine and bisphenol A resin in equal mass ratio.

[0041] 2. The preparation method of the ultra-low density and high strength water-control fracturing proppant is the same as that in Example 1.

[0042] Example 3

[0043] 1. An ultra-low density and high-strength water-control fracturing proppant, the raw materials include a main component and an activator, the main component is composed of fly ash, a binder, a reinforcing agent and a water reducer, and the weight parts of each raw material are as follows: 95 parts of fly ash, 2.8 parts of binder, 2 parts of reinforcing agent, 0.2 parts of polycarboxylic acid water reducer, 15 parts of activator,

[0044] Wherein, the binder is a mixture of carboxymethyl cellulose and liquid epoxy resin in a mass ratio of 0.8:2;

[0045] The enhancer is a mixture of naphthenic crude oil and manganese oxide in equal mass ratio;

[0046] The activator is a mixture of hexamethylenetetramine and bisphenol A resin in equal mass ratio.

[0047] 2. The preparation method of the ultra-low density and high strength water-control fracturing proppant is the same as that in Example 1.

[0048] Example 4

[0049] 1. An ultra-low density and high-strength water-control fracturing proppant, the raw materials include a main component and an activator, the main component is composed of fly ash, a binder, a reinforcing agent and a water reducer, and the weight parts of each raw material are as follows: 91 parts of fly ash, 3.9 parts of binder, 5 parts of reinforcing agent, 0.1 parts of polycarboxylic acid water reducer, 15 parts of activator,

[0050] Wherein, the binder is kaolin;

[0051] The reinforcing agent is nickel-iron slag;

[0052] The activator is a mixture of hexamethylenetetramine and bisphenol A resin in equal mass ratio.

[0053] 2. The method for preparing the ultra-low density and high strength water control fracturing proppant comprises the following steps:

[0054] (1) Material preparation: Prepare the main components, crush and grind the fly ash, pass it through a 200-mesh sieve, and dry it at 105±2℃ for 6h;

[0055] (2) Balling: Fly ash, binder, reinforcing agent and water reducing agent are added into a balling machine for balling at a temperature of 55°C. Water is sprayed continuously during the balling process. The total amount of water sprayed is 10% of the total amount of the main components. Proppant spheres with a particle size of 0.5-0.8 mm are obtained.

[0056] (3) Sintering: Sinter the proppant spheres obtained in step (2) by first heating the temperature to 600°C at 50°C / min, then heating the temperature to 900°C at 60°C / min, and finally heating the temperature to 1200°C at 5°C / min, keeping the temperature for 2 hours, and then cooling to room temperature;

[0057] (4) Activation: The proppant sintered and formed in step (3) is added into a pelletizing machine, and an activator is continuously added during the rolling process of the pelletizing machine to obtain an ultra-low density and high-strength water-controlling fracturing proppant.

[0058] Example 5

[0059] 1. An ultra-low density and high-strength water-control fracturing proppant, the raw materials include a main component and an activator, the main component is composed of fly ash, a binder, a reinforcing agent and a water reducer, and the weight parts of each raw material are as follows: 93.5 parts of fly ash, 1 part of binder, 5 parts of reinforcing agent, 0.5 parts of polycarboxylic acid water reducer, 10 parts of activator,

[0060] Wherein, the binder is clay;

[0061] The reinforcing agent is manganese oxide;

[0062] The activator is a mixture of hexamethylenetetramine and bisphenol A resin in equal mass ratio.

[0063] 2. The method for preparing the ultra-low density and high strength water control fracturing proppant comprises the following steps:

[0064] (1) Material preparation: Prepare the main components, crush and grind the fly ash, pass it through a 200-mesh sieve, and dry it at 105±2℃ for 6h;

[0065] (2) Balling: Fly ash, binder, reinforcing agent and water reducing agent are added into a balling machine for balling at a temperature of 65°C. Water is continuously sprayed during the balling process, and the total amount of water sprayed is 10% of the total amount of the main components to obtain proppant spheres with a particle size of 0.5-0.8 mm.

[0066] (3) Sintering: Sinter the proppant spheres obtained in step (2) by first heating the temperature to 600°C at 50°C / min, then heating the temperature to 900°C at 60°C / min, and finally heating the temperature to 1200°C at 5°C / min, keeping the temperature for 2 hours, and then cooling to room temperature;

[0067] (4) Activation: The proppant sintered and formed in step (3) is added into a pelletizing machine, and an activator is continuously added during the rolling process of the pelletizing machine to obtain an ultra-low density and high-strength water-controlling fracturing proppant.

[0068] Comparative Example

[0069] No activator was added, and the rest was the same as in Example 1.

[0070] Performance Testing

[0071] 1. Measure the volume density (unit: g / cm2) according to SY / T5108-2018 Fracturing Proppant Performance Index and Test Recommended Methods. 3 ), apparent density (unit: g / cm 3 ), breakage rate, water absorption, acid solubility, roundness, sphericity and turbidity;

[0072] 2. The contact angle of distilled water on the proppant surface was measured using a KRUSS DSA100 optical contact angle meter;

[0073] 3. The water blocking ability, i.e., water control ability, of the proppant of the present invention was measured using the water blocking performance measurement method disclosed in "Preparation and Performance of Ultra-low Density Water Control Proppant Based on Hydrophobic Modification" by Shi Bin et al. (Oilfield Chemistry, Vol. 39, No. 3, pp. 401-406);

[0074] The measurement results are shown in Table 1.

[0075] Table 1 Measurement results

[0076]

[0077] According to Table 1 above, the proppants of the present invention and the comparative example both have good roundness, sphericity and low turbidity, but the bulk density and apparent density of the proppants of the present invention are significantly lower than those of the comparative example. It can be seen that the proppants of the present invention have the characteristics of ultra-low density.

[0078] The breakage rate and acid solubility of the proppant of the present invention under the closure pressure (52MPa) are significantly lower than those of the comparative example. It can be seen that the proppant prepared by the present invention has the characteristics of being not easy to break, having high strength, and having good acid resistance and solubility;

[0079] The contact angle and water control height of the proppant of the present invention are significantly higher than those of the comparative example. It can be seen that the proppant prepared by the present invention has good water control ability.

Claims

1. An ultra-low density and high strength water control fracturing proppant, characterized in that: The raw materials of the proppant include a main component and an activator, and the mass ratio of the main component to the activator is 100:(10-15); The main component is composed of the following raw materials in parts by weight based on 100 parts by weight: 91-95 parts of fly ash, 1-4 parts of binder, 2-5 parts of reinforcing agent, and 0.1-0.5 parts of water reducing agent; The activator is a mixture of hexamethylenetetramine and bisphenol A resin; the mass ratio of hexamethylenetetramine to bisphenol A resin is (7-8):7; The binder is any one or any combination of kaolin, clay, carboxymethyl cellulose, and liquid epoxy resin; The reinforcing agent is any one or any combination of nickel iron slag, naphthenic crude oil, and manganese oxide; The proppant is prepared by the following method: (1) Material preparation: prepare the main components, crush and grind the fly ash, pass it through a 200-mesh sieve, and dry it; (2) Balling: Fly ash, binder, reinforcing agent and water reducing agent are added into a balling machine for balling at a temperature of 55-65°C. Water is continuously sprayed during the balling process to obtain proppant spheres with a particle size of 0.5-0.8 mm. (3) Sintering: Sintering the proppant spheres obtained in step (2) and then cooling them to room temperature; The sintering process is as follows: first, the temperature is raised to 600°C at 20-50°C / min, then to 900°C at 30-60°C / min, and finally to 1200°C at 5°C / min, and kept at this temperature for 2h; (4) Activation: The proppant sintered and formed in step (3) is added into a pelletizing machine, and an activator is continuously added during the rolling process of the pelletizing machine to obtain an ultra-low density and high-strength water-controlling fracturing proppant.

2. The ultra-low density and high strength water control fracturing proppant according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.

3. The ultra-low density and high strength water control fracturing proppant according to claim 1, characterized in that: The drying condition in step (1) is drying at 105±2°C for 5-6h.

4. The ultra-low density and high strength water control fracturing proppant according to claim 1, characterized in that: The total amount of water sprayed in step (2) is 10-15% of the total amount of the main components.

Citation Information

Patent Citations

  • Super-hydrophobic propping agent and preparation method

    CN103131406A

  • Coal ash and waste ceramic-prepared petroleum fracturing propping agent and preparation method thereof

    CN103205248A

  • Preparation method of high-volume fly ash ceramsite proppant

    CN103805160A

  • Petroleum proppant and preparation method thereof

    CN104479665A

  • Low-density fly ash fracturing propping agent and preparation method thereof

    CN115141032A