A PMMA compensation film and preparation method thereof

By adding materials such as glutarimide and tougheners to the PMMA compensation film, and adjusting the stretching ratio and film thickness, the problem of TAC compensation film deterioration in high temperature and high humidity environments is solved, and yellow light leakage from IPS panels is eliminated. phenomenon, improving the weather resistance and chemical stability of the film.

CN116120692BActive Publication Date: 2024-10-18ANHUI HEMEI MATERIALS TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211685291.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-10-18
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

The polarization degree of existing TAC compensation films deteriorates in high-temperature or high-humidity environments, resulting in changes in the viewing angle characteristics of IPS panels. In addition, the use of methylene chloride in the production process has environmental issues, and yellow light leakage often occurs.

Method used

PMMA compensation film is used, by adding glutarimide to polymethyl methacrylate, using its positive birefringence to offset the negative birefringence, combining tougheners and compatibilizers, and adjusting the stretch ratio and film thickness. By controlling the in-plane phase difference and thickness phase difference, a compensation film that can improve the yellowish phenomenon is prepared.

Benefits of technology

It effectively eliminates the interference of yellow band light at 45° and 135° side viewing angles of the IPS panel, improves the high temperature resistance and chemical stability of the film, solves the phenomenon of yellow light leakage, and improves the viewing angle performance of the panel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a PMMA compensation film and a preparation method thereof, comprising: 60-80 parts of polymethyl methacrylate, 15-40 parts of glutarimide, 1-10 parts of a toughening agent, and 5-18 parts of a compatibilizer. When the mixture is reacted, the negative birefringence of the polymethyl methacrylate can be offset by the positive birefringence of the glutarimide. By adding a certain weight portion of glutarimide to a common PMMA film preparation material, the positive birefringence of the glutarimide itself is used to offset the negative birefringence of the common polymethyl methacrylate, thereby controlling the refractive index of the material, and then adjusting the thickness of the film by adjusting the stretching ratio. Finally, according to the formula: R0=(n x ‑n y )*d;R th =【(n x +n y ) / 2‑n z 】*dThe in-plane phase difference R0 and the thickness phase difference R th The compensation film is controlled within a certain range to obtain a certain compensation value, which is used to improve the yellowing phenomenon of the IPS panel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of film materials, and in particular to a PMMA compensation film and a preparation method thereof. Background Art

[0002] The IPS hard screen has a stable liquid crystal molecular arrangement structure and a faster response speed, so it has super expressiveness in dynamic clarity. The hard screen also completely eliminates the blur and water ripple diffusion phenomena that occur on traditional LCD screens when subjected to external pressure and shaking. It also eliminates afterimages and tailing when playing high-speed images. While the color expression of the IPS display is linearly improved, it can also intelligently correct the color temperature and white balance to the most accurate color expression, restoring the true colors of the picture to the greatest extent.

[0003] Polarizer is one of the key raw materials of IPS panel. There are two polarizers in the LCD display module, which are respectively attached to the two sides of the glass substrate. Usually, the polarizer structure of IPS panel is PMMA+0-TAC, but TAC polarizing compensation film does not have sufficient heat resistance and moisture resistance. Therefore, the polarization degree of such polarizer will deteriorate under high temperature or high humidity environment, and TAC film will separate from PVA film or the optical properties will deteriorate. The problem of LCD display using such polarizer is that the viewing angle characteristics will change with the change of ambient temperature / humidity, and the deterioration will affect the quality. Secondly, dichloromethane is required in the production process of TAC film, which poses environmental problems.

[0004] In order to solve the above problems, PMMA materials are used in the prior art to replace TAC. PMMA films are transparent, weather-resistant, chemically stable, and have better comprehensive mechanical properties. They can withstand higher tensile, bending, and compression strengths than TAC films. However, the existing PMMA compensation film is a zero birefringence film, and yellow light leakage often occurs when used in IPS panels. For example, R0 is 0±2nm, R th When it is 0±2nm, yellow light leakage will occur at side viewing angles of 45° and 135°.

[0005] Therefore, a PMMA compensation film is now proposed to solve the above problems. Summary of the invention

[0006] The invention overcomes the shortcomings of the prior art and provides a PMMA compensation film and a preparation method thereof.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a PMMA compensation film: comprising the following components in parts by weight: 60 to 80 parts of polymethyl methacrylate, 15 to 40 parts of glutarimide, 1 to 10 parts of a toughening agent, and 5 to 18 parts of a compatibilizer;

[0008] When the mixture is reacted, the negative birefringence of the polymethyl methacrylate can be offset by the positive birefringence of the glutarimide.

[0009] In a preferred embodiment of the present invention, the toughening agent is one or a mixture of two or more of butyl acrylate, methyl acrylate-butadiene-styrene copolymer, ethylene-butyl acrylate-glycidyl methacrylate copolymer, SBS (styrene-butadiene-styrene block copolymer).

[0010] In a preferred embodiment of the present invention, the compatibilizer is one or a mixture of two or more of SBS grafted maleic anhydride, SBS grafted glycidyl methacrylate, SEBS grafted maleic anhydride, and SEBS grafted glycidyl methacrylate.

[0011] In a preferred embodiment of the present invention, the Tg of the PMMA resin is between 115 and 130°C.

[0012] In a preferred embodiment of the present invention, the weight average molecular weight of the polymethyl methacrylate is between 40000-40000-100000.

[0013] In a preferred embodiment of the present invention, a method for preparing a PMMA compensation film comprises the following steps:

[0014] S1. Mixing raw materials: Put 60-80 parts of polymethyl methacrylate, 15-40 parts of glutarimide, 1-10 parts of toughening agent, and 5-18 parts of compatibilizer into a high-speed mixer and stir at high speed;

[0015] S2, granulation: the mixture obtained in step S1 is put into a screw extruder, and extruded and granulated at a temperature of 230-270° C. and an extrusion pressure of 16-25 MPa to obtain PMMA resin particles;

[0016] S3, extrusion calendering: drying the particles obtained in step S2, and then calendering them by an extrusion calendering device to produce a film with a thickness of 0.14 mm to 0.18 mm, and then MD and TD stretching, wherein the MD stretching ratio is 1.0 to 3.5, and the TD stretching ratio is 1.0 to 3.5, and after stretching, a film with a thickness of 0.035 mm to 0.045 mm is obtained.

[0017] According to the formula: R0 = (n x -n y )*d;R th =

(n x +n y ) / 2-n z

[0018] where n x 、ny 、n z represent the refractive index of the x-axis, y-axis, and z-axis respectively, and d represents the film thickness;

[0019] Get R0, R th value.

[0020] In a preferred embodiment of the present invention, in step S1, the raw materials are put into a high-speed mixer and stirred at high speed for 10 minutes to 15 minutes, and the stirring temperature is controlled at 65°C to 75°C to obtain a mixture, and the mixture is cooled to 40°C to 55°C by a cold mixer.

[0021] In a preferred embodiment of the present invention, in step S3, the film is first stretched in MD and then coated with a primer layer online. After drying, the film enters a TD oven for TD stretching, wherein the drying temperature is 80°C to 120°C and the drying time is controlled at 3 to 5 hours.

[0022] In a preferred embodiment of the present invention, in step S3, the extrusion screw temperature of the extrusion calendering equipment is controlled at 250°C to 275°C, the conveying section temperature is controlled at 255°C to 265°C, the extrusion pressure is 6 to 10 MPa, and the extrusion calendering production speed is 16 to 22 m / min.

[0023] In a preferred embodiment of the present invention, the R th The relationship between the value y and the amount of glutarimide added x satisfies: y=ax+b, a is a positive value, b is a negative value, and |b|>ax.

[0024] In a preferred embodiment of the present invention, the in-plane phase difference R0 is -2 to 4 nm, and the thickness phase difference R th It is -8~-2nm.

[0025] In a preferred embodiment of the present invention, the extrusion calendering film forming device in step S3 includes a resin dryer, an extruder, a metal filter, a T-Die, a mirror roller, an MD extension roller, a corona, a coater, a drying machine, a TD extension device, a trimming embossing machine, and a winding machine arranged in sequence.

[0026] In a preferred embodiment of the present invention, the T-Die outlet is located between the first mirror roller and the second mirror roller, the T-Die lip is made of carbon steel treated with tungsten carbide spraying, and the mirror rollers are three smooth rollers of the same diameter fixed on a base, and the surface roughness Ra is less than 0.002 mm.

[0027] The present invention solves the defects existing in the background technology and has the following beneficial effects:

[0028] (1) The present invention adds a certain weight portion of glutarimide to the common PMMA film preparation material, and uses the positive birefringence of glutarimide itself to offset the negative birefringence of common polymethyl methacrylate, thereby controlling the refractive index of the material, and then adjusting the film thickness by adjusting the stretching ratio. Finally, according to the formula: R0 = (n x -n y )*d;R th =

(n x +n y ) / 2-n z

[0029] (2) The present invention adds 15 to 40 parts of glutarimide to 60 to 80 parts of polymethyl methacrylate, controls the MD stretching ratio to 1.0 to 3.5, and the TD stretching ratio to 1.0 to 3.5, and stretches a film with a thickness of 0.035 mm to 0.045 mm, thereby obtaining an in-plane phase difference R0 of -2 to 4 nm and a thickness phase difference R th The compensation film with a thickness of -8 to -2nm can eliminate the interference of yellow band light at the side viewing angles of 45° and 135° of the IPS panel, thereby improving the yellowish phenomenon of the IPS panel at the side viewing angles of 45° and 135°.

[0030] (3) The present invention increases toughness, has outstanding high temperature resistance and good chemical stability by adding toughening agent and compatibilizer to the raw materials for preparing PMMA compensation film, and then designs the production process such as the relative position of T-Die and mirror roller, the roughness of mirror roller, stretching ratio, temperature, etc. to produce a PMMA compensation film with high transparency, high toughness, ultra-thinness and good flatness. DETAILED DESCRIPTION

[0031] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0033] Example 1

[0034] S1. First, the raw materials are mixed: 60 parts of polymethyl methacrylate, 15 parts of glutarimide, 2 parts of toughening agent butyl acrylate, and 5 parts of compatibilizer SBS grafted maleic anhydride are put into a high-speed mixer and stirred at high speed for 10 minutes. The stirring temperature is controlled at 65° C. to obtain a mixture, and the mixture is cooled to 40° C. by a cold mixer;

[0035] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, extruded at a temperature of 240° C. and an extrusion pressure of 18 MPa, and the extrudate is granulated to obtain PMMA resin particles with a Tg of 118° C. for standby use.

[0036] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 80°C, and the drying time is controlled at 5h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.14mm, and then after MD stretching, the primer layer is applied online, and after drying, it enters the TD oven for TD stretching to obtain a film with a thickness of 0.040mm, wherein the extrusion screw temperature is controlled at 250°C, the conveying section temperature is controlled at 255°C, the extrusion pressure is 6MPa, and the extrusion calendering production speed is 16m / min. The MD stretching ratio is 1.8, and the TD stretching ratio is 2.0.

[0037] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0038] Example 2

[0039] S1. First, the raw materials are mixed: 80 parts of polymethyl methacrylate, 40 parts of glutarimide, 8 parts of methyl acrylate-butadiene-styrene copolymer, a toughening agent, and 12 parts of SBS grafted glycidyl methacrylate, a compatibilizer, are put into a high-speed mixer and stirred at high speed for 15 minutes. The stirring temperature is controlled at 75° C. to obtain a mixture, and the mixture is cooled to 45° C. by a cold mixer;

[0040] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 260° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 122° C. for standby use.

[0041] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 100°C, and the drying time is controlled at 4h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.18mm, and then after MD stretching, the primer layer is applied online, and after drying, it enters the TD oven for TD stretching to obtain a film with a thickness of 0.045mm, wherein the extrusion screw temperature is controlled at 265°C, the conveying section temperature is controlled at 258°C, the extrusion pressure is 7MPa, and the extrusion calendering production speed is 18m / min. The MD stretching ratio is 2.0, and the TD stretching ratio is 2.0.

[0042] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0043] Example 3

[0044] S1. First, the raw materials are mixed: 70 parts of polymethyl methacrylate, 20 parts of glutarimide, 5 parts of toughening agent ethylene-butyl acrylate-glycidyl methacrylate, and 17 parts of SEBS grafted maleic anhydride are put into a high-speed mixer and stirred at high speed for 12 minutes. The stirring temperature is controlled at 70° C. to obtain a mixture, and the mixture is cooled to 50° C. by a cold mixer;

[0045] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 250° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 124° C. for standby use.

[0046] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 90°C, and the drying time is controlled at 5h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.18mm, and then stretched in MD, coated with an online primer, dried, and stretched in TD to obtain a film with a thickness of 0.037mm, wherein the extrusion screw temperature is controlled at 260°C, the conveying section temperature is controlled at 255°C, the extrusion pressure is 10MPa, and the extrusion calendering production speed is 22m / min. The MD stretching ratio is 1.8, and the TD stretching ratio is 2.7.

[0047] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0048] Example 4

[0049] S1. First, the raw materials are mixed: 60 parts of polymethyl methacrylate, 20 parts of glutarimide, 3 parts of toughening agent SBS (styrene-butadiene-styrene block copolymer), and 2 parts of SEBS grafted glycidyl methacrylate as a compatibilizer are put into a high-speed mixer and stirred at high speed for 10 minutes. The stirring temperature is controlled at 65° C. to obtain a mixture, and the mixture is cooled to 43° C. by a cold mixer;

[0050] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 260° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 130° C. for standby use.

[0051] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 120°C, and the drying time is controlled at 2h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.18mm, and then stretched in MD, coated with an online primer, dried, and stretched in TD to obtain a film with a thickness of 0.040mm, wherein the extrusion screw temperature is controlled at 260°C, the conveying section temperature is controlled at 255°C, the extrusion pressure is 8MPa, and the extrusion calendering production speed is 16m / min. The MD stretching ratio is 1.8, and the TD stretching ratio is 2.5.

[0052] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0053] Comparative Example 1

[0054] S1. First, the raw materials are mixed: 60 parts of polymethyl methacrylate, 2 parts of glutarimide, 2 parts of toughening agent butyl acrylate, and 5 parts of compatibilizer SBS grafted maleic anhydride are put into a high-speed mixer and stirred at high speed for 10 minutes. The stirring temperature is controlled at 65° C. to obtain a mixture, and the mixture is cooled to 40° C. by a cold mixer;

[0055] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 240° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 118° C. for standby use.

[0056] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 80°C, and the drying time is controlled at 5h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.14mm, and then after MD stretching, the primer layer is applied online, and after drying, it enters the TD oven for TD stretching to obtain a film with a thickness of 0.040mm, wherein the extrusion screw temperature is controlled at 250°C, the conveying section temperature is controlled at 255°C, the extrusion pressure is 6MPa, and the extrusion calendering production speed is 16m / min. The MD stretching ratio is 1.8, and the TD stretching ratio is 2.0.

[0057] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0058] Comparative Example 2

[0059] S1. First, the raw materials are mixed: 80 parts of polymethyl methacrylate, 45 parts of glutarimide, 3 parts of toughening agent SBS (styrene-butadiene-styrene block copolymer), and 12 parts of compatibilizer SBS grafted maleic anhydride are put into a high-speed mixer and stirred at high speed for 15 minutes. The stirring temperature is controlled at 75° C. to obtain a mixture, and the mixture is cooled to 45° C. by a cold mixer;

[0060] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 260° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 122° C. for standby use.

[0061] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 100°C, and the drying time is controlled at 4h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.18mm, and then stretched in MD, coated with an online primer, dried, and stretched in TD to obtain a film with a thickness of 0.060mm, wherein the extrusion screw temperature is controlled at 265°C, the conveying section temperature is controlled at 258°C, the extrusion pressure is 7MPa, and the extrusion calendering production speed is 18m / min. The MD stretching ratio is 1.55, and the TD stretching ratio is 1.93.

[0062] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0063] Comparative Example 3

[0064] S1. First, the raw materials are mixed: 70 parts of polymethyl methacrylate, 30 parts of glutarimide, 5 parts of toughening agent ethylene-butyl acrylate-glycidyl methacrylate, and 17 parts of SEBS grafted maleic anhydride are put into a high-speed mixer and stirred at high speed for 12 minutes. The stirring temperature is controlled at 70° C. to obtain a mixture, and the mixture is cooled to 50° C. by a cold mixer;

[0065] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 280° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 124° C. for standby use.

[0066] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 90°C, and the drying time is controlled at 5h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.18mm, and then stretched in MD, coated with an online primer, dried, and stretched in TD to obtain a film with a thickness of 0.037mm, wherein the extrusion screw temperature is controlled at 285°C, the conveying section temperature is controlled at 280°C, the extrusion pressure is 10MPa, and the extrusion calendering production speed is 22m / min. The MD stretching ratio is 1.8, and the TD stretching ratio is 2.7.

[0067] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0068] Comparative Example 4

[0069] S1. First, the raw materials are mixed: 90 parts of polymethyl methacrylate, 28 parts of glutarimide, 3 parts of toughening agent SBS (styrene-butadiene-styrene block copolymer), and 12 parts of compatibilizer SBS grafted maleic anhydride are put into a high-speed mixer and stirred at high speed for 15 minutes. The stirring temperature is controlled at 75° C. to obtain a mixture, and the mixture is cooled to 45° C. by a cold mixer;

[0070] S2. Next, granulation: the mixture obtained in step S1 is put into a screw extruder, and the extrudate is granulated at a temperature of 260° C. and an extrusion pressure of 18 MPa to obtain PMMA resin particles with a Tg of 122° C. for standby use.

[0071] S3, extrusion calendering: drying the raw material particles obtained in step S2, the drying temperature is 100°C, and the drying time is controlled at 4h; after drying, the raw material particles are extruded by an extruder, passed through a metal filter to T-Die, and the molten blend resin flowing out of the lip falls between the first mirror roller and the second mirror roller, and is calendered by the first mirror roller, the second mirror roller, and the third mirror roller to produce a film with a thickness of 0.18mm, and then stretched in MD, coated with an online primer, dried, and stretched in TD to obtain a film with a thickness of 0.060mm, wherein the extrusion screw temperature is controlled at 265°C, the conveying section temperature is controlled at 258°C, the extrusion pressure is 7MPa, and the extrusion calendering production speed is 18m / min. The MD stretching ratio is 1.55, and the TD stretching ratio is 1.93.

[0072] S4, finished product winding: the biaxially oriented film obtained in step S3 is wound up to obtain a finished product after trimming and embossing.

[0073] Table 1: Performance table

[0074]

[0075] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

[0076] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A PMMA compensation film, characterized in that: The invention comprises the following components in parts by weight: 60 to 80 parts of polymethyl methacrylate, 15 to 40 parts of glutarimide, 1 to 10 parts of toughening agent, and 5 to 18 parts of compatibilizer; wherein: when the polymethyl methacrylate is 60 to 70 parts, the glutarimide is 15 to 20 parts; when the polymethyl methacrylate is 70 to 80 parts, the glutarimide is 20 to 40 parts; When the above mixture reacts, the negative birefringence of the polymethyl methacrylate can be offset by the positive birefringence of the glutarimide; The PMMA compensation film is prepared by the following method: S1. Mixing raw materials: Put 60-80 parts of polymethyl methacrylate, 15-40 parts of glutarimide, 1-10 parts of toughening agent, and 5-18 parts of compatibilizer into a high-speed mixer and stir at high speed; S2, granulation: the mixture obtained in step S1 is put into a screw extruder, and extruded and granulated at a temperature of 230-270° C. and an extrusion pressure of 16-25 MPa to obtain PMMA resin particles; S3, extrusion calendering: drying the particles obtained in step S2, and then calendering them by an extrusion calendering device to produce a film with a thickness of 0.14 mm to 0.18 mm, and then MD and TD stretching, wherein the MD stretching ratio is 1.0 to 3.5, and the TD stretching ratio is 1.0 to 3.5, and after stretching, a film with a thickness of 0.035 mm to 0.045 mm is obtained; According to the formula: R0=(n x -n y )*d; R th =【(n x +n y ) / 2-n z 】*d, Where n x 、n y 、n z represent the refractive index of the x-axis, y-axis, and z-axis respectively, and d represents the film thickness; Get R0, R th The in-plane phase difference R0 is -2 to 4 nm, and the thickness phase difference R th It is -8~-2nm.

2. A PMMA compensation film according to claim 1, characterized in that: The toughening agent is one or a mixture of two or more of butyl acrylate, methyl acrylate-butadiene-styrene copolymer, ethylene-butyl acrylate-glycidyl methacrylate copolymer, and SBS (styrene-butadiene-styrene block copolymer).

3. The PMMA compensation film according to claim 1, characterized in that: The compatibilizer is one of SBS grafted maleic anhydride, SBS grafted glycidyl methacrylate, SEBS grafted maleic anhydride, and SEBS grafted glycidyl methacrylate, or a mixture of two or more thereof.

4. The PMMA compensation film according to claim 1, characterized in that: The Tg of the PMMA resin is between 115 and 130°C.

5. The PMMA compensation film according to claim 1, characterized in that: The weight average molecular weight of the polymethyl methacrylate is between 40,000 and 100,000.

6. The PMMA compensation film according to claim 1, characterized in that: The extrusion calendering equipment in step S3 includes a resin dryer, an extruder, a metal filter, a T-Die, a mirror roller, an MD stretching roller, a corona, a coater, a dryer, a TD stretching device, a trimming embossing device, and a winding machine arranged in sequence.

7. The PMMA compensation film according to claim 6, characterized in that: The T-Die outlet is located between the first mirror roller and the second mirror roller. The T-Die lip is made of carbon steel treated with tungsten carbide spraying. The mirror rollers are three smooth rollers of the same diameter fixed on a base, and the surface roughness Ra is less than 0.002mm.

Citation Information

Patent Citations

  • Resin composition, and molded article and film thereof