A kind of heat-insulating polyester fiber and preparation method thereof
By combining modified silica gel particles with polyurethane resin, the problems of easy damage to the polyester fiber insulation film and anti-fraction difference of the sandwich structure are solved, and the long-term thermal insulation and mechanical properties of polyester fiber are improved. .
Patent Information
- Application Number
- CN202211706148.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The thermal insulation film of polyester fiber is prone to breakage and fall off during wear and washing, and the flexural resistance of the sandwich structure is poor, resulting in a short-lasting thermal insulation performance.
Modified silica gel particles were used to prepare porous silicon gel by sol gel method and coated with polyurethane foam resin, and combined with a compatibilizer to improve the thermal insulation and mechanical properties of polyester fibers.
It significantly improves the thermal insulation performance of polyester fiber, so that it still has excellent thermal insulation performance after multiple uses, and improves mechanical properties to prevent the insulation from falling off and wear.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of textiles, and more specifically, to a heat-insulating polyester fiber and a preparation method thereof. Background Art
[0002] Polyester fiber is a synthetic fiber made by polycondensation of organic dibasic acid and diol. Polyester fiber itself does not have thermal insulation properties. Therefore, in the related technology, silica aerogel is used to modify polyester fiber so that polyester fiber fabric has certain thermal insulation properties.
[0003] The industry generally uses the following two methods to improve the thermal insulation performance of polyester fibers: First, silica aerogel is made into a coating agent and applied to the surface of polyester fibers. Silica aerogel forms a thermal insulation film on the surface of polyester fibers, making the polyester fibers have thermal insulation performance. However, the thermal insulation performance of polyester fiber fabrics obtained by this method is not long-lasting. In a short period of time, during wearing and washing, the thermal insulation film on the surface is easily damaged and falls off, and the thermal insulation performance of polyester fiber fabrics is not long-lasting.
[0004] The second method is to fill silica aerogel between two polyester fiber fabrics to make a thermal insulation fabric with a "polyester fiber fabric layer-silica gel layer-polyester fiber fabric layer" structure. However, the thermal insulation fabric with this sandwich structure has poor folding resistance, and the silica gel layer is very brittle. After folding, the silica gel is easy to powder and escape from the gaps in the polyester fiber fabric layer, resulting in the polyester fiber fabric's thermal insulation performance not being durable.
[0005] In view of the above situation, there is an urgent need in the art to develop a polyester fiber with long-term thermal insulation performance, so that the fabric made of the polyester fiber still has excellent thermal insulation performance after repeated use. Summary of the invention
[0006] In order to solve the problem that polyester fibers are difficult to have long-term thermal insulation performance, the present application provides a thermal insulation polyester fiber and a preparation method thereof.
[0007] In a first aspect, the present application provides a heat-insulating polyester fiber, which adopts the following technical solution:
[0008] A heat-insulating polyester fiber is made of the following raw materials in parts by weight:
[0009] 100 parts of polyester masterbatch;
[0010] 2.8 to 14.6 parts of compatibilizer;
[0011] 18.4 to 42.2 parts of modified silica gel particles;
[0012] Additives 0.003-0.01 parts;
[0013] The preparation method of the modified silica gel particles comprises the following steps:
[0014] The porous silica gel is obtained by a sol-gel method, the porous silica gel is crushed and the water content is controlled to be 10wt% to 30wt%;
[0015] Adding porous silica gel into polyol, the weight ratio of porous silica gel to polyol is 1:(12.5-16), mixing well, and obtaining reactant 1;
[0016] Then, diisocyanate and catalyst are added to reactant 1, wherein the weight ratio of polyol to diisocyanate is controlled to be (12.5-16):(4-7.5), and the mixture is stirred and reacted for 30s-60s. After the reaction, the mixture is aged and crushed to obtain modified silica gel particles.
[0017] By adopting the above technical scheme, the modified silica gel particles prepared in the present application have a core-shell structure, and the modified silica gel particles use porous silica gel as the core; at the same time, the moisture contained in the porous silica gel can be used as a foaming agent in the subsequent preparation steps, so that the surface of the porous silica gel is coated with a polyurethane foaming resin.
[0018] Compared with traditional unmodified silica aerogel, modified silica gel particles for modifying polyester resin have the following advantages: First, the surface of the porous silica gel in this application is coated with a layer of high-density foam polyurethane material. At the same volume, the air content of the modified silica gel particles is higher than that of traditional silica aerogel, which can effectively reduce the heat transfer coefficient of polyester fibers, thereby significantly improving the thermal insulation performance of polyester fibers.
[0019] Second, polyurethane materials have good compatibility with polyester materials. Under the action of the compatibilizer, the modified silica gel particles can be fully dispersed in the polyester resin. On the one hand, the thermal insulation performance of the polyester fiber is uniform, and it has long-term thermal insulation performance. On the other hand, while increasing the addition amount of modified silica gel particles, the possibility of stress concentration points in the polyester fiber is reduced, thereby improving the mechanical properties of the polyester fiber.
[0020] Third, the polyurethane material limits the movement of the porous silicone gel, preventing the porous silicone gel from migrating to the surface of the polyester fiber. It can also protect the porous silicone gel and reduce the possibility of wear and fall off of the porous silicone gel during long-term use, thereby enabling the polyester fiber to have long-lasting thermal insulation properties.
[0021] In summary, the use of a compatibilizer and modified silica gel particles to jointly modify the polyester masterbatch in the present application can significantly improve the thermal insulation performance of the polyester fiber, and the thermal insulation performance is long-lasting.
[0022] Optionally, the weight ratio of the porous silicone gel to the polyol is 1:(13-15).
[0023] By adopting the above technical solution, the polyol includes but is not limited to polyether polyol and polyester polyol, and polyester polyol is preferred in this application. In this application, the weight ratio of porous silicone gel and polyol is controlled so that the polyol fully infiltrates the surface of porous silicone gel while ensuring that the porosity of porous silicone gel is maintained within a certain range and the air content is still moderate.
[0024] Preferably, the weight ratio of the polyol to the diisocyanate is (13-15):(4.5-5).
[0025] By adopting the above technical solution, the diisocyanate includes but is not limited to toluene diisocyanate. The weight ratio of polyol and diisocyanate is adjusted to make the cell density of the foamed polyurethane material on the surface of the modified silica gel particles more dense, so that the air content of the modified silica gel particles is further improved, thereby promoting the further improvement of the thermal insulation performance of the polyester fiber.
[0026] Optionally, the particle size of the modified silica gel particles is between 10 and 200 μm.
[0027] By adopting the above technical solution, the particle size of the modified silica gel particles is controlled, so that the mechanical properties of the polyester fiber are excellent, and the thermal insulation durability of the polyester fiber is further improved.
[0028] Optionally, the polyester masterbatch is polytrimethylene terephthalate.
[0029] By adopting the above technical solution, polyester masterbatch includes but is not limited to polyethylene terephthalate (PET) and polytrimethylene terephthalate (PTT). Compared with PET, PTT has better toughness and elasticity, which can make the thermal insulation polyester fiber have better mechanical properties.
[0030] Optionally, the compatibilizer is one or more of polyethylene grafted with maleic anhydride, polyolefin elastomer grafted with maleic anhydride, and polypropylene grafted with maleic anhydride.
[0031] By adopting the above technical scheme, the polar segments contained in polyethylene grafted with maleic anhydride, polyolefin elastomer grafted with maleic anhydride, and polypropylene grafted with maleic anhydride play a role of promoting capacity. At the same time, the alkane segments can also play a toughening role, which can effectively make up for the toughness loss caused by the modified silica gel particles, making it difficult for the polyester fiber to be locally broken when repeatedly folded, thereby making the polyester fiber have long-lasting thermal insulation properties.
[0032] Preferably, the compatibilizer is polypropylene grafted with maleic anhydride.
[0033] By adopting the above technical solution, compared with polyethylene grafted with maleic anhydride and polyolefin elastomer grafted with maleic anhydride, polypropylene grafted with maleic anhydride has the best toughening effect on polyester fiber within this addition amount range.
[0034] Preferably, the weight ratio of the compatibilizer to the polyester masterbatch is (5-10):100.
[0035] By adopting the above technical solution, the amount of the compatibilizer added not only has a great influence on the toughness of the polyester fiber, but also has a certain influence on the heat resistance of the polyester fiber. Therefore, within this addition amount range, the polyester fiber can have both excellent toughness and heat resistance.
[0036] Optionally, the auxiliary agent includes an antioxidant.
[0037] By adopting the above technical scheme, antioxidants include but are not limited to Basf330, Basf1010, Basf1076. Antioxidants can effectively improve the anti-yellowing performance of polyester fibers, reduce the possibility of yellowing of polyester fibers caused by compatibilizers such as polyethylene grafted maleic anhydride, polyolefin elastomer grafted maleic anhydride, and polypropylene grafted maleic anhydride; and also reduce the possibility of ester bond breakage in polyester fibers, making polyester fibers less prone to degradation and yellowing, and having better durability in use.
[0038] In a second aspect, the present application provides a method for preparing a heat-insulating polyester fiber, using the following technical solution:
[0039] A method for preparing a heat-insulating polyester fiber comprises the following steps: weighing a polyester masterbatch, a compatibilizer, modified silica gel particles and an auxiliary agent according to weight parts, adding the compatibilizer, modified silica gel particles and the auxiliary agent after the polyester masterbatch is melted, and extruding to obtain the heat-insulating polyester fiber.
[0040] In summary, this application has the following beneficial effects:
[0041] 1. The present application adopts modified silica gel particles and a compatibilizer to modify the thermal insulation performance of polyester masterbatch, and uses a compatibilizer to promote the compatibility of the modified silica gel particles with the polyester masterbatch. Since the modified silica gel particles have a high air content and a low heat transfer coefficient, the thermal insulation performance of the polyester fiber can be effectively improved. In addition, the modified silica gel particles have good stability in the polyester fiber and are not easy to fall off from the polyester fiber, so that the polyester fiber has long-term thermal insulation performance.
[0042] 2. In the present application, a specific compatibilizer is selected. The polar segments contained in polyethylene grafted with maleic anhydride, polyolefin elastomer grafted with maleic anhydride, and polypropylene grafted with maleic anhydride play a role in promoting compatibilization. At the same time, the introduced alkane segments can also play a toughening role, which can effectively compensate for the toughness loss caused by the modified silica gel particles, making it difficult for the polyester fiber to be partially broken when repeatedly folded, thereby making the polyester fiber have long-lasting thermal insulation properties. DETAILED DESCRIPTION
[0043] The present application is further described in detail below in conjunction with preparation examples and embodiments.
[0044] Unless otherwise specified, the raw material specifications used in the following preparation examples, examples and comparative examples are as follows;
[0045] Polyester masterbatch: PET: Brand: Eastman TM F61HC;
[0046] PTT: Brand 3030G NC010;
[0047] Polyol: polyether polyol, brand: polyether 330.
[0048] Polyester polyol, brand: AD-60;
[0049] Polyethylene grafted with maleic anhydride: Brand: Plas-Easy TM A1068;
[0050] Polyolefin elastomer grafted with maleic anhydride: Brand: Plas-Easy™ A2361;
[0051] Polypropylene grafted with maleic anhydride: Brand: Plas-Easy™ A1028.
[0052] Preparation Example of Modified Silica Gel Particles
[0053] Preparation Example 1
[0054] A modified silica gel particle is prepared according to the following steps:
[0055] 1 kg of ethyl orthosilicate, 2 kg of ethanol and 2 kg of deionized water were mixed, oxalic acid was added to adjust the pH value to 2.5, and hydrolysis was performed for 3 hours; 0.01 kg of 3-aminopropyltrihydroxysilane was added, stirred, and ammonia water was added to adjust the pH value to 9, and the reaction was performed for 2 hours to obtain a porous silica gel; the porous silica gel was placed in a 55°C environment and sealed for aging for 45 hours; the porous silica gel was crushed and dried at 55°C until the water content in the porous silica gel was 10wt%;
[0056] Weigh 12.5 kg of polyether 330 and 4 kg of toluene diisocyanate, dry them for later use;
[0057] 1 kg of porous silica gel and 0.001 kg of stannous octoate were added to polyether 330, and stirred to obtain reactant 1;
[0058] Toluene diisocyanate was added to reactant 1, stirred at a speed of 3000 rpm, reacted at 25°C for 10 seconds after stirring, sent to a maturation tunnel for maturation at 60°C for 48 hours, and ground in a grinder to a particle size of 5 to 10 μm to obtain modified silica gel particles.
[0059] Preparation Example 2-7
[0060] A modified silica gel particle, which is different from Preparation Example 1 in that the weight ratio of porous silica gel, polyether 330, and toluene diisocyanate is different, and the specific weight ratio is shown in Table 1 below:
[0061] Table 1. Weight of porous silicone gel, polyether 330, and toluene diisocyanate
[0062] Components Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Preparation Example 5 Preparation Example 6 Preparation Example 7 Porous silicone gel / kg 1 1 1 1 1 1 1 Polyether 330 / kg 12.5 16 13 15 15 15 15 Toluene diisocyanate / kg 4 4 4 4 7.5 4.5 5 Stannous octoate / kg 0.001 0.001 0.001 0.001 0.001 0.001 0.001
[0063] Preparation Example 8
[0064] A modified silica gel particle, which is different from Preparation Example 7 in that polyester polyol AD-60 of equal mass is used instead of polyether 330.
[0065] Preparation Example 9
[0066] A modified silica gel particle, which is different from Preparation Example 8 in that the water content of the porous silica gel is controlled at 20wt%.
[0067] Preparation Example 10
[0068] A modified silica gel particle, which is different from Preparation Example 8 in that the water content of the porous silica gel is controlled at 30wt%.
[0069] Preparation Example 11
[0070] A modified silica gel particle, which is different from Preparation Example 9 in that toluene diisocyanate is added to reactant 1, stirred at a speed of 1500 rpm, and reacted at 25° C. for 30 seconds after stirring.
[0071] Preparation Example 12
[0072] A modified silica gel particle, which is different from Preparation Example 9 in that the particle size of the modified silica gel particle is 200-500 μm.
[0073] Preparation Example 13
[0074] A modified silica gel particle, which is different from Preparation Example 9 in that the particle size of the modified silica gel particle is 10 to 200 μm.
[0075] Preparation Comparative Example
[0076] Preparation Comparative Example 1
[0077] A silica gel particle is prepared according to the following steps:
[0078] Take 1kg of ethyl orthosilicate, 2kg of ethanol and 2kg of deionized water, mix them, add oxalic acid to adjust the pH value to 2.5, and hydrolyze for 3 hours; then add 0.01kg of 3-aminopropyltrihydroxysilane, stir, add ammonia water to adjust the pH value to 9, react for 2 hours, and obtain silica gel particles; place the porous silica gel in a 55°C environment and seal it for 45 hours of aging; after crushing the silica gel particles, dry them at 55°C until the moisture content is ≤1%.
[0079] Preparation Comparative Example 2
[0080] A modified silica gel particle, which is different from Preparation Example 1 in that the water content of the porous silica gel is controlled at 5wt%.
[0081] Preparation Comparative Example 3
[0082] A modified silica gel particle, which is different from Preparation Example 1 in that the water content of the porous silica gel is controlled at 50wt%.
[0083] Preparation Comparative Example 4
[0084] A modified silica gel particle, which is different from Preparation Example 1 in that the weights of porous silica gel, polyether 330, and toluene diisocyanate are different. The specific weight ratio is as follows: the weights of porous silica gel, polyether 330, and toluene diisocyanate are 1:5:2.5. Example
[0085] Example 1
[0086] A thermal insulation polyester fiber is prepared according to the following steps:
[0087] Take 10kg polyester masterbatch Eastman TM F61HC is put into the drum, the steam valve and the vacuum pump are opened, dried, crystallized and melted to obtain polyester raw materials;
[0088] Then take 0.28kg of polyolefin elastomer grafted with maleic anhydride Plas-Easy TM A2361, 1.84 kg of modified silica gel particles obtained in Preparation Example 1 and 30 g of antioxidant Basf168 were added to the polyester raw material and blended. The blend was transported to a spinning assembly, extruded, spun, blown and cooled, oiled, drawn and wound to obtain a heat-insulating polyester fiber with a single-filament fineness of 1.7 dtex;
[0089] Among them, in the air blowing cooling step, the wind pressure is 200Pa, the wind speed is 0.5m / s, the wind temperature is 18°C, and the wind humidity is 70%.
[0090] Example 2-13
[0091] A heat insulating polyester fiber, which is different from Example 1 in that the source of the modified silica gel particles is different, and the specific source is shown in Table 2 below:
[0092] Table 2. Sources of modified silica gel particles
[0093] project Modified silica gel particles project Modified silica gel particles Example 2 Preparation Example 2 Example 8 Preparation Example 8 Example 3 Preparation Example 3 Example 9 Preparation Example 9 Example 4 Preparation Example 4 Example 10 Preparation Example 10 Example 5 Preparation Example 5 Embodiment 11 Preparation Example 11 Example 6 Preparation Example 6 Example 12 Preparation Example 12 Example 7 Preparation Example 7 Example 13 Preparation Example 13
[0094] Embodiment 14
[0095] A heat-insulating polyester fiber, which differs from Example 13 in that the compatibilizer is selected differently and the same mass of Plas-Easy TM A1068 replaces Plas-Easy TM A2361.
[0096] Embodiment 15
[0097] A heat-insulating polyester fiber, which differs from Example 13 in that the compatibilizer is selected differently and the same mass of Plas-Easy TM A1028 replaces Plas-Easy TM A2361.
[0098] Example 16
[0099] A heat insulating polyester fiber, which is different from Example 15 in that the weight ratio of the compatibilizer to the polyester masterbatch is 5:100.
[0100] Embodiment 17
[0101] A heat insulating polyester fiber, which is different from Example 15 in that the weight ratio of the compatibilizer to the polyester masterbatch is 10:100.
[0102] Embodiment 18
[0103] A heat insulating polyester fiber, which is different from Example 15 in that the weight ratio of the compatibilizer to the polyester masterbatch is 14.6:100.
[0104] Embodiment 19
[0105] A heat insulating polyester fiber, which is different from Example 17 in that the weight ratio of modified silica gel particles to polyester masterbatch is 25.3:100.
[0106] Embodiment 20
[0107] A heat insulating polyester fiber, which differs from Example 17 in that the weight ratio of modified silica gel particles to polyester masterbatch is 36.6:100.
[0108] Embodiment 21
[0109] A heat insulating polyester fiber, which is different from Example 17 in that the weight ratio of modified silica gel particles to polyester masterbatch is 42.2:100.
[0110] Embodiment 22
[0111] A heat insulating polyester fiber, which differs from Example 20 in that the weight ratio of antioxidant Basf168 to polyester masterbatch is 0.01:100.
[0112] Embodiment 23
[0113] A heat-insulating polyester fiber, which is different from Example 22 in that the type of polyester masterbatch is different, and 3030G NC010 of the same quality is used instead of Eastman TM F61HC.
[0114] Comparative Example
[0115] Comparative Examples 1-4
[0116] A heat insulating polyester fiber, which is different from Example 1 in that the source of the modified silica gel particles is different, and the specific source is as follows:
[0117] Table 3. Sources of modified silica gel particles
[0118] project Source of Antimicrobial Masterbatch Comparative Example 1 Preparation Comparative Example 1 Comparative Example 2 Preparation Comparative Example 2 Comparative Example 3 Preparation Comparative Example 3 Comparative Example 4 Preparation Comparative Example 4
[0119] Comparative Example 5
[0120] A heat insulating polyester fiber, which differs from Example 1 in that polyester masterbatch of equal quality is used instead of the compatibilizer Plas-Easy™ A2361.
[0121] Comparative Example 6
[0122] A heat insulating polyester fiber, which differs from Example 1 in that polyester masterbatch of equal mass is used to replace the compatibilizer Plas-Easy™ A2361, and silica gel particles of equal mass prepared in Preparation Comparative Example 1 are used to replace the modified silica gel particles prepared in Preparation Example 1.
[0123] Detection Methods
[0124] The polyester fiber yarns prepared in Examples 1-23 and Comparative Examples 1-6 were respectively made into polyester fiber fabrics of 190T (T: warp and weft density) and a specification of 200mm×50mm, and the following tests were performed.
[0125] Thermal insulation performance: Refer to the method of GB / T 11048-2018 to test the heat transfer coefficient of polyester fiber fabrics. The lower the heat transfer coefficient, the better the thermal insulation performance;
[0126] Durability: Refer to the method of GB / T 3921-2008, wash the polyester fiber fabric 100 times, and then refer to the method of GB / T11048-2018 to test the heat transfer coefficient of the fabric;
[0127] Mechanical properties: The breaking strength and breaking elongation of polyester fiber were tested according to ASTM D638 to characterize the mechanical properties of polyester fiber;
[0128] Yellowing resistance level: After the yellowing resistance test Suntest, the color change of the sample before and after the test is compared and divided into 1-5 levels. The best level is 5, which means basically no color change; 4, which means slight color change; 3, which means light color change; 2, which means obvious color change; 1, which means serious color change.
[0129] The specific test results are shown in Table 4 below:
[0130] Table 4. Performance test
[0131] sample <![CDATA[Heat transfer coefficient (×10 -3 W / m·K)]]> <![CDATA[Heat transfer coefficient after 100 washings (×10 -3 W / m·K)]]> Elongation at break (%) Breaking strength(MPa) Anti-yellowing grade Example 1 8.765 9.648 88.5 77.0 3 Example 2 8.756 9.634 88.7 77.7 3 Example 3 8.744 9.616 88.8 78.6 3 Example 4 8.695 9.543 89.6 82.3 3 Example 5 8.668 9.502 90.0 84.3 3 Example 6 8.643 9.465 90.4 86.3 3 Example 7 8.635 9.453 90.5 86.9 3 Example 8 8.628 9.442 90.6 87.4 3 Example 9 8.604 9.406 90.9 89.3 3 Example 10 8.595 9.393 91.1 90.0 3 Embodiment 11 8.618 9.427 90.7 88.2 3 Example 12 8.583 9.375 91.3 80.9 3 Example 13 8.588 9.382 91.2 90.5 3 Embodiment 14 8.540 9.310 91.9 94.3 3 Embodiment 15 8.528 9.292 92.1 95.3 4 Example 16 8.525 9.288 92.1 95.5 4 Embodiment 17 8.517 9.276 92.2 96.1 4 Embodiment 18 8.520 9.280 92.2 95.9 4 Embodiment 19 8.477 9.216 92.8 99.3 4 Embodiment 20 8.438 9.157 93.4 102.5 4 Embodiment 21 8.500 9.250 92.5 97.5 4 Embodiment 22 8.497 9.246 92.5 101.7 5 Embodiment 23 8.144 9.288 112.8 104.1 5 Comparative Example 1 8.977 10.954 85.3 61.6 3 Comparative Example 2 9.035 11.070 84.5 57.6 3 Comparative Example 3 8.900 10.800 86.5 67.1 3 Comparative Example 4 8.948 10.896 85.8 63.7 3 Comparative Example 5 8.944 12.488 73.8 13.5 4 Comparative Example 6 8.765 9.648 88.5 77.0 3
[0132] Combining Example 1 and Comparative Examples 1 and 6 with Table 4, it can be seen that in Comparative Examples 1 and 6, conventional porous silica gel is added to the polyester masterbatch, and the heat transfer coefficient of the polyester fiber is much higher than that of Example 1. Therefore, it is proved that the modification of the porous silica gel by foaming polyurethane in the present application can effectively reduce the heat transfer coefficient of the polyester fiber.
[0133] The modified silica gel particles used in Comparative Examples 2 and 3 both form a polyurethane foam resin layer on the surface of the porous silica gel, but the heat transfer coefficients of both are much higher than that of Example 1, indicating that the water content of the porous silica gel has a significant effect on the foamed polyurethane of its outer layer. Too much or too little water content affects the foaming effect of the polyurethane, resulting in an increase in its heat transfer coefficient instead of a decrease, and the thermal insulation performance of the polyester fiber deteriorates.
[0134] Although a polyurethane foam resin layer is also formed on the surface of the porous silicone gel in Comparative Example 4, the low amount of polyol added results in limited increase in the air content in the modified silica gel particles, which is still far lower than that in Example 1, resulting in a slight improvement in thermal insulation performance.
[0135] In Comparative Example 5, no compatibilizer is used, resulting in poor compatibility between the modified silica gel particles and the polyester masterbatch, which is easily lost during the washing process, making it difficult for the polyester fiber fabric prepared in Comparative Example 5 to have long-term thermal insulation performance.
[0136] Therefore, the heat transfer coefficient of the polyester fiber obtained in Example 1 is only 8.675×10 -3 W / m•K. After washing a hundred times, the heat transfer coefficient did not increase significantly, indicating that the modified silica gel particles and the compatibilizer can work together to improve the thermal insulation and long-term thermal insulation properties of polyester fibers.
[0137] In combination with Examples 1-13 and Table 4, the porous silicone gel, the weight ratio between the polyol and the diisocyanate, and the selection of the polyol all have a significant effect on the thermal insulation properties of the polyester fiber, and can effectively reduce the heat transfer coefficient of the polyester fiber.
[0138] In combination with Examples 19-21 and Table 4, the addition amount of modified silica gel particles is controlled within the range of 18wt% to 25wt%, which can optimize the thermal insulation and mechanical properties of the polyester fiber.
[0139] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A thermal insulation polyester fiber, Features: Made from the following raw materials in parts by weight: 100 parts of polyester masterbatch; 2.8 to 14.6 parts of compatibilizer; 18.4 to 42.2 parts of modified silica gel particles; Additives 0.003-0.01 parts; The preparation method of the modified silica gel particles comprises the following steps: The porous silica gel is obtained by a sol-gel method, the porous silica gel is crushed and the water content is controlled to be 10wt% to 30wt%; Adding porous silica gel into polyol, the weight ratio of porous silica gel to polyol is 1:(12.5-16), mixing well, and obtaining reactant 1; Then, diisocyanate and catalyst are added to reactant 1, wherein the weight ratio of polyol to diisocyanate is controlled to be (12.5-16):(4-7.5), and the mixture is stirred and reacted for 10-30 seconds. After the reaction, the mixture is aged and crushed to obtain modified silica gel particles.
2. The heat insulating polyester fiber according to claim 1, Features: The weight ratio of the porous silica gel to the polyol is 1:(13-15).
3. The heat insulating polyester fiber according to claim 2, Features: The weight ratio of the polyol to the diisocyanate is (13-15):(4.5-5).
4. The heat insulating polyester fiber according to claim 1, Features: The particle size of the modified silica gel particles is between 10 and 200 μm.
5. The heat insulating polyester fiber according to claim 1, Features: The polyester masterbatch is polytrimethylene terephthalate.
6. The heat insulating polyester fiber according to claim 1, Features: The compatibilizer is one or more of polyethylene grafted with maleic anhydride, polyolefin elastomer grafted with maleic anhydride, and polypropylene grafted with maleic anhydride.
7. The heat insulating polyester fiber according to claim 6, Features: The compatibilizer is polypropylene grafted with maleic anhydride.
8. The heat insulating polyester fiber according to claim 6, Features: The weight ratio of the compatibilizer to the polyester masterbatch is (5-10):
100.
9. The heat insulating polyester fiber according to claim 6, Features: The auxiliary agent includes an antioxidant.
10. A method for preparing a heat insulating polyester fiber according to any one of claims 1 to 9, Features: The steps include: The polyester masterbatch, the compatibilizer, the modified silica gel particles and the additives are weighed in parts by weight, the compatibilizer, the modified silica gel particles and the additives are added after the polyester masterbatch is melted, and the heat insulating polyester fiber is obtained by extrusion.