A method for preparing polymer foam using polymer solution in high-pressure gas
By preparing polymer solution foam in high-pressure gas and controlling the pore size using a three-dimensional network structure and auxiliary solvent, the foaming problem of polymers with strong intermolecular forces was solved, and stable foams with enhanced functionality were prepared at low temperature.
Patent Information
- Application Number
- CN202310164689.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-26
AI Technical Summary
Existing high-pressure gas foaming methods are difficult to effectively prepare polymer foams rich in active functional groups such as hydroxyl, carboxyl, or amino groups. This is because these polymers have strong intermolecular forces that restrict molecular chain movement, which hinders gas dissolution, diffusion, and cell growth. Furthermore, traditional plasticizers have limited modification effects, and high processing temperatures can easily lead to polymer degradation.
A method for preparing foam using polymer solution in high-pressure gas involves degassing followed by gas permeation in an autoclave. Temperature and pressure are controlled to allow polymer molecules to form a three-dimensional network structure. Foaming is then achieved through depressurization or heating, with the addition of auxiliary solvents and functional fillers to regulate the cell structure.
It significantly reduces the foaming temperature, increases the solubility of gas in the polymer matrix, forms a stable cell structure, and achieves lightweight and functionalized materials. The process is simple and controllable and applicable to a variety of polymer materials.
Smart Images

Figure CN116141566B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer foam material preparation, and relates to a method for preparing polymer foam by utilizing polymer solution in high-pressure gas. Background Art
[0002] Polymer foam materials have the characteristics of large specific surface area, high damping and light weight. They are widely used in aerospace, bioengineering, water treatment, heat insulation, shock absorption and lightweight components. At present, there are mechanical foaming, chemical foaming and physical foaming methods for preparing polymer foam. Mechanical foaming refers to the use of mechanical stirring to fully mix air and matrix, and then fix the pores through curing molding, but this method has the disadvantage of high equipment requirements; chemical foaming refers to the use of interaction between polymer components to generate gas or thermal decomposition of the foaming agent in the matrix to generate gas, but the prepared foam often has residual foaming agent, which will have a certain impact on the performance and environment of the product; physical foaming refers to the use of changes in the foaming environment to cause the foaming agent in the matrix to undergo phase change to form pores. Among them, the high-pressure gas foaming method in the physical foaming method is widely used in the preparation of foam products because of the characteristics of no reagent residue in the product, wide source of foaming agent and low price.
[0003] The high-pressure gas foaming method is a method of placing a polymer material in a high-pressure gas environment for swelling and plasticization, and then by quickly releasing the pressure or increasing the temperature, the gas in the polymer reaches a thermodynamically unstable state, rapidly nucleates and grows, and obtains a foam product. It is worth noting that in the high-pressure gas foaming process, the growth of the pores is based on the movement of the molecular chain segments. There is a class of polymers rich in active functional groups such as hydroxyl, carboxyl or amino groups, such as cellulose and its derivatives, chitin, polyvinyl alcohol and polyacrylamide. There are strong intermolecular forces between these functional groups, including van der Waals forces and hydrogen bonds, which limit the mobility of the molecular chain or form highly crystalline regions, hindering the dissolution, diffusion, nucleation and pore growth of the gas. In addition, polymers with strong intermolecular forces are difficult to be thermoplastically molded under mild conditions. Therefore, it is difficult to achieve lightweighting of such materials using traditional high-pressure gas foaming technology. Although the addition of plasticizers can weaken the intermolecular forces in such materials to a certain extent, increase the solubility of the gas, and reduce the processing temperature of the polymer. However, so far, the modification effect of plasticizers is not significant, and the modified polymer still requires a higher processing temperature to achieve foaming, which can easily cause polymer degradation. Summary of the invention
[0004] In response to the technical difficulties encountered when foaming polymers with strong intermolecular forces in high-pressure gas, the present invention provides a method for preparing polymer foams using a polymer solution in high-pressure gas, so as to enhance the mobility of the molecular chain segments of the polymer, lower the foaming temperature, reduce the resistance of the gas entering the polymer matrix, and increase the solubility of the gas in the polymer matrix, while ensuring that a stable pore structure can be formed during the preparation.
[0005] To achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0006] A method for preparing polymer foam using a polymer solution in high-pressure gas comprises the following steps:
[0007] (1) degassing a polymer solution to obtain a casting solution; the polymer solution is a homogeneous solution, or a homogeneous solution containing a crosslinking agent, wherein the homogeneous solution is formed by dissolving a polymer in a solvent; the polymer can be crosslinked to form a three-dimensional network structure under the temperature T of the autoclave in step (2), or the polymer can react with the crosslinking agent to form a three-dimensional network structure under the temperature T of the autoclave in step (2);
[0008] (2) casting a casting liquid into a mold, placing the mold in an autoclave, introducing a gas into the autoclave to act as a physical foaming agent, controlling the temperature in the autoclave to be T and the pressure in the autoclave to be P, the gas swells and penetrates the casting liquid in the mold, and a polymer in the casting liquid, or a polymer and a cross-linking agent, undergo a cross-linking reaction during the swelling and penetration process. When the polymer molecules form a three-dimensional network structure, foaming is performed by a pressure relief method or a temperature increase method;
[0009] (3) vacuum drying the foamed product obtained in step (2) to obtain a polymer foam.
[0010] In step (2) of the above technical solution, the preferred temperature T of the autoclave is 20 to 170° C. and the pressure P is 0.2 to 30 MPa.
[0011] In step (2) of the above technical solution, the swelling and penetration time is controlled to ensure that the polymer forms a three-dimensional network structure during the swelling and penetration process. Usually, the swelling and penetration time is 5 to 1440 minutes.
[0012] In the above technical solution, in order to further increase the pore size and expansion ratio of the foam material, in step (2), an auxiliary solvent is added to the autoclave before the gas is introduced into the autoclave. The auxiliary solvent is the solvent used to prepare the homogeneous solution or is the main component of the solvent. During the preparation process of step (2), the casting liquid in the mold does not contact the liquid auxiliary solvent.
[0013] Furthermore, in the above technical solution, the amount of the auxiliary solvent added to the autoclave in step (2) is 0.5% to 80% of the volume of the autoclave.
[0014] In step (2) of the above technical solution, after the casting liquid is cast into the mold, the depth of the casting liquid in the mold is at least 2 mm.
[0015] In the above technical solution, the polymer material in the homogeneous solution can be one or more than one; when the homogeneous solution contains two or more polymer materials, polymer materials that can undergo cross-linking reactions with each other can be selected to prepare polymer foam without or with the addition of a cross-linking agent, or multiple polymer materials that cannot undergo cross-linking reactions with each other can be selected to prepare polymer foam with the addition of a cross-linking agent. When the homogeneous solution contains two or more polymer materials, the prepared foam is a composite polymer foam.
[0016] In the above technical solution, there are no special requirements for the type of polymer used to prepare the homogeneous solution except that it can be dissolved in an appropriate solvent to form a homogeneous solution and can undergo cross-linking reaction between polymers or between polymers and cross-linking agents to form a three-dimensional network. For example, feasible polymers include at least one of chitosan and its derivatives, sodium alginate and its derivatives, starch and its derivatives, cellulose and its derivatives, hyaluronic acid, polyvinyl alcohol, polyacrylic acid, polyacrylamide or polyethylene glycol, and can also be other polymers that meet the above two requirements.
[0017] In the above technical solution, the content of the polymer in the casting liquid is preferably 1 wt.% to 60 wt.%. When the casting liquid contains a crosslinking agent, the mass of the crosslinking agent in the casting liquid usually does not exceed 150 wt.% of the mass of the polymer.
[0018] Furthermore, in the above technical solution, the cross-linking agent is a multifunctional organic or inorganic cross-linking agent, for example, common cross-linking agents include malic acid, glutaraldehyde, citric acid and boric acid.
[0019] In the above technical solution, the solvent is one or more of water, alkaline solvent, acidic solvent and organic solvent. It is worth noting that chemical reaction should not occur between the components in the mixed solvent. The organic solvent includes one or more of ethanol, glycerol, dimethyl sulfoxide and tetrahydrofuran.
[0020] In the above technical scheme, according to different application requirements, the polymer solution of step (1) may also contain fillers, and the mass of the fillers in the polymer solution is usually no more than 50wt.% of the mass of the polymer in the polymer solution. Because the molecular segments in the polymer solution have strong mobility, fillers that can interact with the polymer groups can be selected, which is conducive to the dispersion of the fillers in the solution, and then the functionalization of the polymer foam is easily realized, giving the polymer foam catalysis, electromagnetic shielding, water treatment and antibacterial functions. The filler can be a nano-scale filler or a micron-scale filler, and the specific type and size of the filler can be selected according to the actual application requirements with reference to the fillers in the existing polymer composite materials. For example, common fillers include graphene, carbon nanotubes, carbon nanofibers, graphite, fillers with catalytic functions (such as nano gold, silver, palladium, etc.), hydrophilic / hydrophobic fillers, and vitamins.
[0021] In the above technical solution, the gas introduced into the autoclave is one or a mixed gas of more than one of carbon dioxide, nitrogen, air, helium or lower alkanes.
[0022] The present invention uses a polymer solution to prepare a polymer foam in a high-pressure gas, and the change process of the polymer solution is mainly as follows:
[0023] The present invention utilizes high-pressure gas to foam the polymer solution. When the high-pressure gas swells and penetrates the polymer solution, the polymer molecular chains gradually form a three-dimensional network through a cross-linking reaction, and then the gas in the polymer solution rapidly nucleates and grows through a pressure release method or a temperature increase method, and finally forms a polymer foam. Specifically:
[0024] During the foaming process of polymer solution by high-pressure gas, the three-dimensional network structure of the polymer is an important factor affecting the growth and stability of the pores. The molecular chain segments in the polymer solution have strong mobility, so that the gas molecules dissolved in the polymer solution can overcome the energy barrier of pore growth and grow rapidly under mild conditions. When the swelling and penetration time is short, the three-dimensional network structure of the system is still imperfect. At this time, the gas in the matrix can nucleate and grow, but because the molecular chain segments have strong mobility and are not restricted by the three-dimensional network structure, the molecular chains are prone to slip, resulting in the pore structure formed by foaming being unable to maintain its own stability and collapsing; as the swelling and penetration time increases, the three-dimensional network structure of the system gradually improves. At this time, the molecular chain segments still have strong mobility, but the movement of the molecular chains is restricted by the three-dimensional network structure and cannot slip, thus maintaining the stability of the pore structure after foaming.
[0025] Compared with the prior art, the technical solution provided by the present invention produces the following beneficial technical effects:
[0026] 1. The present invention provides a method for preparing polymer foam using polymer solution in high-pressure gas. The method proposes for the first time to use polymer solution as a substrate for high-pressure gas foaming, which can significantly reduce the foaming temperature of the material, thereby preparing polymer foam material under mild conditions. In particular, it provides an effective way to foam polymer materials rich in active functional groups such as hydroxyl, carboxyl or amino groups, and can solve the problem that such materials have strong intermolecular forces or form highly crystalline regions, which limit the mobility of molecular chains and hinder the dissolution, diffusion, nucleation and cell growth of gases.
[0027] 2. In the method provided by the present invention, the solvent not only helps to improve the solubility of the gas in the polymer matrix, but also acts as a physical foaming agent, increasing the total amount of the foaming agent in the matrix, so that the foam material prepared by the method has a larger pore size and a lower sample density, and can be used for lightweight materials or thermal insulation materials, etc.
[0028] 3. The foaming matrix used in the method of the present invention is a polymer solution. Since the molecular segments in the polymer solution have strong mobility, it is beneficial to the dispersion of functional fillers. At the same time, the hydroxyl, carboxyl, amino and other functional groups on the polymer can interact with the functional fillers to anchor the functional fillers, further improving the stability of the functional fillers in the polymer foam matrix.
[0029] 4. The method of the present invention can further increase the cell size and foaming ratio by adding the solvent used in preparing the homogeneous solution or the main component of the solvent as an auxiliary solvent to the autoclave before the gas is introduced into the autoclave, and controlling the casting liquid in the mold not to contact the liquid auxiliary solvent during the swelling and penetration process. At the same time, by adjusting the type of foaming gas, foaming method, swelling and penetration temperature and pressure, type and amount of crosslinking agent and other conditions, the cell size and morphology of the polymer foam can be regulated.
[0030] 5. The method of the present invention has simple process, good process controllability, wide gas source and good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a scanning electron microscope image of the cross section of the polyvinyl alcohol (PVA) foam prepared in Example 1 without adding an auxiliary solvent.
[0032] Figure 2 This is a scanning electron microscope image of the cross section of the PVA foam prepared in Example 2 with the addition of an auxiliary solvent.
[0033] Figure 3 This is a scanning electron micrograph of the cross section of the chitosan (CS) foam prepared in Example 3 without adding an auxiliary solvent.
[0034] Figure 4 This is a scanning electron microscope image of the cross section of the CS foam prepared in Example 4 with the addition of an auxiliary solvent.
[0035] Figure 5 This is a scanning electron micrograph of a cross section of a PVA foam loaded with silver nanoparticles prepared in Example 5 without adding an auxiliary solvent. DETAILED DESCRIPTION
[0036] The following examples further illustrate the method for preparing polymer foam using polymer solution in high pressure gas provided by the present invention. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention according to the above invention content and implement them specifically, which still falls within the scope of protection of the present invention.
[0037] Example 1
[0038] In this embodiment, PVA foam is prepared using a PVA solution in a high pressure carbon dioxide (HPCD) environment, and the steps are as follows:
[0039] (1) PVA is added to distilled water and stirred in a water bath at 95° C. until the PVA is completely dissolved to form a PVA homogeneous solution; the cross-linking agent citric acid is fully dissolved in distilled water to form a citric acid solution; the PVA homogeneous solution and the citric acid solution are evenly mixed, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of PVA is 15 wt.%, and the mass of citric acid is 80 wt.% of the mass of PVA.
[0040] (2) Casting liquid is cast into a mold and placed in an autoclave, CO2 gas is introduced into the autoclave as a physical foaming agent, and the temperature in the autoclave is controlled to be 110°C and the pressure is 10MPa. At this time, CO2 gas swells and penetrates the casting liquid in the mold, and the PVA in the casting liquid and the cross-linking agent undergo a cross-linking reaction during the swelling and penetration process. When the swelling and penetration time is 80 minutes, CO2 gas reaches saturation in the casting liquid and PVA forms a three-dimensional network structure under the action of citric acid. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked PVA matrix.
[0041] (3) The foamed product obtained in step (2) is vacuum dried at 80° C. to obtain PVA foam.
[0042] The diameter of the PVA foam prepared in this embodiment is about 13 mm. The interaction between water molecules and PVA molecules in the solution weakens the interaction between PVA molecules, so that the crystalline area in the PVA material is dissolved. Figure 1It can be seen that low-density PVA foam is obtained at 110°C, and the processing temperature is low, which is beneficial to reducing the energy consumption of foam material production. Figure 1 As shown. During the foaming process, the water in the solution not only helps to further increase the solubility of the gas in the matrix, but also acts as a physical foaming agent in the foaming process. Therefore, the cell size of the PVA foam is large, and the density of the sample is 0.25g / cm 3 .
[0043] Example 2
[0044] In this embodiment, PVA foam is prepared using a PVA solution in an HPCD environment, and a solvent is added to the autoclave during the preparation process to assist in foaming, and the steps are as follows:
[0045] (1) PVA is added to distilled water and stirred in a water bath at 95° C. until the PVA is completely dissolved to form a PVA homogeneous solution; the cross-linking agent citric acid is fully dissolved in distilled water to form a citric acid solution; the PVA homogeneous solution and the citric acid solution are evenly mixed, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of PVA is 15 wt.%, and the mass of citric acid is 80 wt.% of the mass of PVA.
[0046] (2) Cast the casting liquid in the mold and place it in an autoclave, then add 2% of the volume of distilled water into the autoclave, making sure that the distilled water does not contact the casting liquid in the mold, then introduce CO2 gas into the autoclave as a physical foaming agent, and control the temperature in the autoclave to be 110°C and the pressure to be 10MPa. At this time, the CO2 gas swells and penetrates the casting liquid in the mold, and the PVA in the casting liquid and the cross-linking agent undergo a cross-linking reaction in this process. When the swelling and penetration time is 120 minutes, the CO2 gas reaches saturation in the casting liquid and the PVA forms a three-dimensional network structure under the action of citric acid. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked PVA matrix.
[0047] During the preparation process of step (2), the casting liquid in the mold never contacts the liquid distilled water in the autoclave.
[0048] (3) The foamed product obtained in step (2) is vacuum dried at 80° C. to obtain PVA foam.
[0049] The diameter of the PVA foam prepared in this embodiment is about 25 mm. The scanning electron microscope image of the cross section of the PVA foam prepared in this embodiment is as follows: Figure 2As shown. Compared with Example 1, in Example 2, distilled water is introduced into the autoclave to assist foaming during the saturation of the casting liquid. The presence of distilled water can inhibit the transfer of water molecules on the surface of the casting liquid to HPCD, maintain the distance between molecular chains in the PVA solution, and thus make step (2) require a longer swelling and penetration time to form a complete three-dimensional network structure, but maintain the cross-linking balance of the solution system, so that the pore size of the material is more uniform. At the same time, the introduction of distilled water into the autoclave inhibits the transfer of water molecules in the casting liquid to the environment, increases the content of foaming agent in the casting liquid, and further increases the pore size of the PVA foam. The sample density is 0.051g / cm 3 .
[0050] Example 3
[0051] In this embodiment, CS foam is prepared using CS solution in a HPCD environment, and the steps are as follows:
[0052] (1) CS was added to an acetic acid solution with a mass fraction of 1.50 wt.%, and stirred at room temperature until CS was completely dissolved to form a CS homogeneous solution; the cross-linking agent citric acid was fully dissolved in distilled water to form a citric acid solution; the CS homogeneous solution and the citric acid solution were mixed evenly, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of CS was 6 wt.%, and the mass of citric acid was 66.7 wt.% of the mass of CS.
[0053] (2) The casting liquid is cast into a mold and placed in an autoclave. CO2 gas is introduced into the autoclave as a physical foaming agent. The temperature in the autoclave is controlled to be 60°C and the pressure is controlled to be 10 MPa. At this time, the CO2 gas swells and penetrates the casting liquid in the mold, and the CS molecules in the casting liquid and the cross-linking agent undergo a cross-linking reaction during the swelling and penetration process. When the swelling and penetration time is 120 minutes, the CO2 gas reaches saturation in the casting liquid and the CS forms a three-dimensional network structure under the action of citric acid. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked CS matrix.
[0054] (3) The foamed product obtained in step (2) is dried under vacuum at 40° C. to obtain CS foam.
[0055] The diameter of the CS foam prepared in this example is about 12 mm. The scanning electron microscope image of the cross section of the CS foam prepared in this example is as follows: Figure 3 The polymer substrate used in this embodiment is CS which is only soluble in acidic solution. CS foam can be prepared by high pressure gas foaming method by adjusting the process conditions. CS foam is prepared at a mild temperature in this embodiment. The pore size is relatively large and the sample density is 0.36 g / cm 3 .
[0056] Example 4
[0057] In this embodiment, CS foam is prepared by using CS solution in HPCD environment, and a solvent is added to the autoclave to assist foaming during the preparation process, and the steps are as follows:
[0058] (1) CS was added to an acetic acid solution with a mass fraction of 1.50 wt.%, and stirred at room temperature until CS was completely dissolved to form a CS homogeneous solution; the cross-linking agent citric acid was fully dissolved in distilled water to form a citric acid solution; the CS homogeneous solution and the citric acid solution were mixed evenly, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of CS was 6 wt.%, and the mass of citric acid was 66.7 wt.% of the mass of CS.
[0059] (2) The casting liquid is cast into a mold and placed in an autoclave, and then 2% of the volume of the autoclave is added to the autoclave. Note that the distilled water does not contact the casting liquid in the mold. Then, CO2 gas is introduced into the autoclave as a physical foaming agent, and the temperature in the autoclave is controlled to be 60°C and the pressure is controlled to be 10MPa. At this time, the CO2 gas swells and penetrates the casting liquid in the mold, and the CS in the casting liquid and the cross-linking agent undergo a cross-linking reaction during the swelling and penetration process. When the swelling and penetration time is 150 minutes, the CO2 gas reaches saturation in the casting liquid and the CS forms a three-dimensional network structure under the action of citric acid. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked CS matrix.
[0060] During the preparation process of step (2), the casting liquid in the mold never contacts the liquid distilled water in the autoclave.
[0061] (3) The foamed product obtained in step (2) is vacuum dried at 40° C. to obtain PVA foam.
[0062] The diameter of the CS foam prepared in this example is about 22 mm. The scanning electron microscope image of the cross section of the CS foam prepared in this example is as follows: Figure 4 Compared with Example 3, distilled water was introduced into the autoclave to assist foaming during the swelling and infiltration process, which further increased the cell size of the CS foam and the sample density was 0.098 g / cm 3 .
[0063] Example 5
[0064] In this embodiment, PVA foam loaded with silver nanoparticles is prepared using a PVA solution in a high-pressure nitrogen environment, and the steps are as follows:
[0065] (1) PVA and silver nitrate are added to distilled water, and stirred in a water bath at 95° C. until PVA is completely dissolved to form a homogeneous PVA solution containing silver nitrate; sodium borohydride is added to the homogeneous PVA solution containing silver nitrate, and stirred in a water bath at 60° C. until the mixture is uniformly mixed; citric acid, a crosslinking agent, is fully dissolved in distilled water to form a citric acid solution; the PVA solution containing silver nitrate and sodium borohydride is uniformly mixed with the citric acid solution, and air bubbles are removed by centrifugation to obtain a casting solution; in the casting solution, the concentration of PVA is 17.6 wt.%, the mass of citric acid is 66.7 wt.% of the mass of PVA, the mass of silver nitrate is 4.6 wt.% of the mass of PVA, and the mass of sodium borohydride is 0.1 wt.% of the mass of PVA.
[0066] (2) Casting liquid is cast into a mold and placed in an autoclave, and nitrogen is introduced into the autoclave as a physical foaming agent, and the temperature in the autoclave is controlled to be 110°C and the pressure is controlled to be 10MPa. At this time, nitrogen swells and penetrates the casting liquid in the mold, and the PVA in the casting liquid and the cross-linking agent undergo a cross-linking reaction during the swelling and penetration process. When the swelling and penetration time is 90 minutes, CO2 gas reaches saturation in the casting liquid and PVA forms a three-dimensional network structure under the action of citric acid. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked PVA matrix.
[0067] (3) The foamed product obtained in step (2) is vacuum dried at 80° C. to obtain PVA foam loaded with silver nanoparticles.
[0068] The diameter of the PVA foam prepared in this example is about 15 mm. The scanning electron microscope image of the cross section of the PVA foam loaded with silver nanoparticles prepared in this example is as follows: Figure 5 As shown, the sample density is 0.32 g / cm 3 .
[0069] Example 6
[0070] In this embodiment, sodium alginate (SA) foam is prepared using a sodium alginate (SA) solution in a high-pressure nitrogen environment, and the steps are as follows:
[0071] (1) SA is added to distilled water and stirred until SA is completely dissolved to form a SA homogeneous solution; malic acid, a cross-linking agent, is fully dissolved in distilled water to form a malic acid solution; the SA homogeneous solution and the malic acid solution are evenly mixed, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of SA is 10 wt.%, and the mass of malic acid is 80 wt.% of the mass of SA.
[0072] (2) The casting liquid is cast into a mold and placed in an autoclave, and nitrogen is introduced into the autoclave as a physical foaming agent. The temperature in the autoclave is controlled to be 100°C and the pressure is controlled to be 12 MPa. At this time, the nitrogen swells and penetrates the casting liquid in the mold, and the SA in the casting liquid and the cross-linking agent undergo a cross-linking reaction during the swelling and penetration process. When the swelling and penetration time is 80 minutes, the nitrogen reaches saturation in the casting liquid and the SA forms a three-dimensional network structure under the action of malic acid. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked SA matrix.
[0073] (3) The foamed product obtained in step (2) was dried under vacuum at 80° C. to obtain SA foam.
[0074] Example 7
[0075] In this embodiment, SA foam is prepared by the same operation as in Example 6, except that in step (2), after the mold is placed in the autoclave, distilled water (20% of the volume of the autoclave) is added to the autoclave, and it is noted that the distilled water does not contact the casting liquid in the mold, and during the preparation process of step (2), the casting liquid in the mold does not contact the liquid distilled water in the autoclave.
[0076] Example 8
[0077] In this embodiment, a mixed solution of PVA and CS was used to prepare PVA-CS composite foam in an HPCD environment, and the steps were as follows:
[0078] (1) PVA was added to distilled water, and stirred in a water bath at 95° C. until PVA was completely dissolved to form a PVA homogeneous solution; CS was added to an acetic acid solution with a mass fraction of 1.50 wt.%, and stirred at room temperature until CS was completely dissolved to form a CS homogeneous solution; and citric acid, a cross-linking agent, was fully dissolved in distilled water to form a citric acid solution;
[0079] The PVA homogeneous solution, the CS homogeneous solution and the citric acid solution are uniformly mixed, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of PVA is 12wt.%, the concentration of CS is 4wt.%, and the mass of citric acid is 70wt.% of the sum of the masses of PVA and CS.
[0080] (2) The casting liquid cast in the mold is placed in an autoclave, and CO2 gas is introduced into the autoclave as a physical foaming agent. The temperature in the autoclave is controlled to be 30°C and the pressure is 5MPa. At this time, the CO2 gas swells and penetrates the casting liquid in the mold, and the PVA, CS and citric acid in the casting liquid undergo a cross-linking reaction during the swelling and penetration process. When the swelling and penetration time is 1080min, the CO2 gas reaches saturation in the casting liquid and PVA and CS form a three-dimensional network structure under the action of citric acid. Then, the pressure is reduced to normal pressure at a rate of 1MPa / s, and the sample is placed in an 80°C oil bath for foaming for 3min.
[0081] (3) The foamed product obtained in step (2) is vacuum dried at 80° C. to obtain a PVA-CS composite foam.
[0082] Example 9
[0083] In this example, PVA-CS composite foam was prepared by the same operation as in Example 8, except that in step (2), after the mold was placed in the autoclave, an acetic acid solution of 10% of the volume of the autoclave was added to the autoclave, and it was noted that the acetic acid solution did not contact the casting liquid in the mold, and during the preparation process of step (2), the casting liquid in the mold did not contact the liquid acetic acid solution in the autoclave.
[0084] Example 10
[0085] In this embodiment, a mixed solution of PVA and polyacrylic acid (PAA) is used to prepare PVA-PAA composite foam in a high-pressure butane environment, and the steps are as follows:
[0086] (1) PVA was added to distilled water, and stirred in a water bath at 95° C. until PVA was completely dissolved to form a homogeneous PVA solution; PAA was added to the above homogeneous PVA solution, stirred and mixed evenly, and then centrifuged to remove bubbles to obtain a casting solution; in the casting solution, the concentration of PVA was 8 wt.%, and the concentration of PAA was 8 wt.%.
[0087] (2) The casting liquid is cast into a mold and placed in an autoclave, butane gas is introduced into the autoclave as a physical foaming agent, and the temperature in the autoclave is controlled to be 90°C and the pressure is controlled to be 12MPa. At this time, the butane gas swells and penetrates the casting liquid in the mold, and the groups on the PVA and PAA molecular chains in the casting liquid undergo cross-linking reactions during the swelling and penetration process. When the swelling and penetration time is 180 minutes, the butane gas reaches saturation in the casting liquid and the PVA and PAA cross-linking reaction forms a three-dimensional network structure. The pressure in the autoclave is reduced to normal pressure by the pressure relief method to foam the cross-linked PVA-PAA matrix.
[0088] (3) The foamed product obtained in step (2) is vacuum dried at 80° C. to obtain a PVA-PAA composite foam.
[0089] Embodiment 11
[0090] In this embodiment, PVA-PAA composite foam was prepared by the same operation as in Example 10, except that in step (2), after placing the mold in the autoclave, 15% of the volume of the autoclave was added to the autoclave. Note that the distilled water did not contact the casting liquid in the mold, and during the preparation process of step (2), the casting liquid in the mold did not contact the liquid distilled water in the autoclave.
Claims
1. A method for preparing polymer foam using a polymer solution in a high pressure gas, characterized in that: The following steps are involved: (1) degassing the polymer solution to obtain a casting solution; the polymer solution is a homogeneous solution, or a homogeneous solution containing a crosslinking agent, and the homogeneous solution is formed by dissolving a polymer in a solvent; the polymer can be crosslinked to form a three-dimensional network structure under the temperature T of the autoclave in step (2), or the polymer can be crosslinked with the crosslinking agent to form a three-dimensional network structure under the temperature T of the autoclave in step (2); (2) Casting the casting liquid into a mold, placing the mold in an autoclave, introducing gas into the autoclave as a physical foaming agent, controlling the temperature in the autoclave to be T and the pressure to be P, the gas swells and penetrates the casting liquid in the mold, and the polymer in the casting liquid, or the polymer and the cross-linking agent, undergo a cross-linking reaction during the swelling and penetration process. When the polymer molecules form a three-dimensional network structure, foaming is performed by a pressure relief method or a temperature increase method; In this step, the temperature T of the autoclave is controlled to be 20~170 o C. The pressure P is 0.2~30 MPa, and the time of controlling swelling and penetration is 5~1440 min; (3) vacuum drying the foamed product obtained in step (2) to obtain a polymer foam; In step (2), before the gas is introduced into the autoclave, an auxiliary solvent is added into the autoclave. The auxiliary solvent is the solvent used in preparing the homogeneous solution or is the main component of the solvent. During the preparation process of step (2), the casting liquid in the mold does not contact with the liquid auxiliary solvent.
2. The method for preparing polymer foam using a polymer solution in high pressure gas according to claim 1, characterized in that: The amount of auxiliary solvent added to the autoclave in step (2) is 0.5% to 80% of the volume of the autoclave.
3. The method for preparing polymer foam using a polymer solution in high pressure gas according to claim 1, characterized in that: The homogeneous solution contains one or more polymers.
4. The method for preparing polymer foam using a polymer solution in high pressure gas according to claim 1, characterized in that: The content of the polymer in the casting liquid is 1 wt.%~60 wt.%. When the casting liquid contains a cross-linking agent, the mass of the cross-linking agent in the casting liquid does not exceed 150 wt.% of the mass of the polymer.
5. The method for preparing polymer foam using a polymer solution in high pressure gas according to claim 1, characterized in that: The polymer solution in step (1) also includes fillers, and the mass of the fillers in the polymer solution does not exceed 50 wt.% of the mass of the polymer.
6. The method for preparing polymer foam using a polymer solution in high pressure gas according to claim 1, characterized in that: The solvent is one or a combination of water, alkaline solvent, acidic solvent and organic solvent, and no chemical reaction should occur between the components in the mixed solvent.
7. The method for preparing polymer foam using a polymer solution in high pressure gas according to claim 1, characterized in that: The gas introduced into the autoclave is one or a mixture of more than one of carbon dioxide, nitrogen, air, helium or lower alkanes.
Citation Information
Patent Citations
One-step preparation method of light high-strength microsphere phenolic resin-based foamy carbon
CN110921648A
Gas-liquid two-phase self-balancing supercritical swelling foaming method
CN113134934A