A formula and preparation method of sandstone glaze for ceramic ware surface
By using sand and gravel glaze with silver-carried titanium dioxide composite powder on the surface of ceramic ware, the problem of bacterial adhesion on the surface of ceramics is solved, the antibacterial performance and aesthetic effect of the glaze are achieved, and the cleanliness and health of ceramic products are improved.
Patent Information
- Application Number
- CN202310069231.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-02-06
AI Technical Summary
The pores on the surface of ceramic products make bacteria easy to adhere, affecting the cleanliness and beauty of the ceramics, and posing a threat to human health. The existing glaze lacks effective antibacterial properties.
A formula of sand and gravel glaze on the surface of ceramic ware, including potassium feldspar, kaolin, calcium carbonate, talc powder, quartz sand and other raw materials, is made into a slurry by grinding, and silver-carrying titanium dioxide composite powder is added, and the oxidation and firing is carried out. The technology forms antibacterial glaze, controlling the heating rate and firing temperature to enhance the mechanical strength and antibacterial properties of the glaze surface.
The prepared glaze not only has a similar matte effect and a special glossy appearance, but also provides significant antibacterial properties by loading silver ions, which can effectively prevent bacteria from adhesion, improve the cleanliness and aesthetics of the ceramic surface, and ensure human health.
Smart Images

Figure BDA0004063673960000071 
Figure BDA0004063673960000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic production, and in particular relates to a formula and a preparation method of aventurine glaze for the surface of ceramic ware. Background Art
[0002] Glaze is a colorless or colored glassy thin layer covering the surface of ceramic products. It is made of mineral raw materials (feldspar, quartz, talc, kaolin, etc.) and other mineral raw materials in a certain proportion (some raw materials can be made into frits first) and ground into glaze slurry, applied to the surface of the body, and calcined at a certain temperature. It can increase the mechanical strength, thermal stability and dielectric strength of the product, and also has the characteristics of beautifying objects, easy to wipe, and not being corroded by dust and filth. There are many types of glazes. According to the body type, there are porcelain glaze, pottery glaze and flint glaze; according to the firing temperature, it can be divided into high-temperature glaze, medium-temperature glaze and low-temperature glaze; according to the appearance characteristics, it can be divided into transparent glaze, opaque glaze, colored glaze, glossy glaze, matte glaze, crack glaze (craze), frosted glaze, crystalline glaze, etc.; according to the composition of glaze, it can be divided into lime glaze, feldspar glaze, lead glaze, lead-free glaze, boron glaze, lead-boron glaze, etc.
[0003] The microstructure of ceramic materials is composed of crystal phase, glass phase and pores. The final product has a porosity of 5% to 10%. If these pores are exposed to the outside, a large number of bacteria will adhere to them. Under the action of various physical or chemical forces such as van der Waals force, capillary force, hydrogen bond, etc., these bacteria are easy to accumulate on the surface concave and convex parts or enter the micropores, causing the surface of the ceramic to change color, seriously affecting the cleanliness and beauty of the ceramic surface. Tableware and cups used in the home are the most used ceramic products in life. A large number of bacteria attached to the surface of household ceramic products will cause certain harm to the human body and threaten human health. Therefore, a glaze with antibacterial effect is urgently needed to enhance the antibacterial effect of ceramic glaze. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a formula and preparation method of sandstone glaze for the surface of ceramic utensils.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A formula for a sandstone glaze for the surface of ceramic ware, comprising the following raw materials in parts by weight: 20-35 parts of potassium feldspar, 3-5 parts of kaolin, 10-12 parts of calcium carbonate, 7-10 parts of talc, 5-10 parts of dolomite, 25-50 parts of quartz sand, 5-8 parts of barium carbonate, 2-5 parts of zirconium silicate, 1-3.5 parts of aluminum oxide, and 5-10 parts of composite powder;
[0007] The surface of the ceramic ware is made of sandstone glaze comprising the following steps:
[0008] Mix the raw materials of various components according to the formula and add them into a grinding jar to form dry powder. Add 45-50% water by weight of the dry powder and grind for 10-12 hours. During the grinding process, the ratio of material, ball and water is controlled to be 1:1.2:0.5. After the grinding, a slurry is formed, which is sieved to remove iron and the concentration is adjusted to a true specific gravity of 52-54 degrees. It is then coated on the surface of ceramic utensils, dried and sent to the kiln for oxidation firing. After natural cooling, it is taken out of the kiln to obtain sandstone glaze.
[0009] Furthermore, the oxidation sintering is divided into three stages: the first stage: room temperature to 650°C, controlling the heating rate at 3°C / min; the second stage: 650-850°C, controlling the heating rate at 3.5°C / min; the third stage: 850-1100°C, controlling the heating rate at 2°C / min, and keeping the highest temperature for 15 minutes.
[0010] Furthermore, the coating thickness is controlled to be 1-2.5 mm.
[0011] Furthermore, the composite powder is prepared by the following steps:
[0012] Step S1, adding urea to deionized water, stirring and adding polyvinyl pyrrolidone, stirring evenly, adding a 0.01-0.1 mol / L sodium chloride solution (preferably a 0.05 mol / L sodium chloride solution), stirring evenly, adding a defoamer, slowly dropping a 0.01-0.1 mol / L silver nitrate solution (preferably a 0.05 mol / L silver nitrate solution) while stirring, stirring at a uniform speed and reacting (preferably 1-3 h) after the addition is completed, adding a mass fraction of 5-15% (preferably 10%) titanyl sulfate and a mass fraction of 10-20% (preferably 15%) zirconium sulfate solution to obtain a mixed solution, and controlling the amount ratio of urea, polyvinyl pyrrolidone, sodium chloride solution, defoamer, silver nitrate solution and deionized water to be 3-5 g: 0.1-0.2 g: 20-22 mL: 0.05-0.08 g: 20 mL: 100 mL;
[0013] Step S2, heating the mixed solution to 70-95° C. (preferably 90° C.), keeping the temperature for reaction (preferably 4 hours), cooling to room temperature after the reaction is completed, slowly dripping a 6-10% (preferably 8%) sodium hydrogen phosphate aqueous solution by mass, stirring at a uniform speed and reacting (preferably reacting for 2 hours), vacuum filtering after the reaction is completed, washing the filter cake three times with deionized water and anhydrous ethanol in sequence, drying and calcining after washing to obtain a composite powder, and controlling the amount of sodium hydrogen phosphate aqueous solution to be 8-12% of the volume of the mixed solution.
[0014] In step S1, urea is used as a precipitant, and silver ions and chloride ions are reacted to generate silver chloride precipitates through a combination of uniform precipitation and coprecipitation. The formed silver chloride is used as a seed crystal, and titanium oxysulfate is hydrolyzed under alkaline conditions to form titanium hydroxide deposited on the surface of the silver chloride crystals. Phosphate ions are then added to precipitate zirconium ions and titanium ions, and finally calcined to form a composite powder, which is a silver-loaded titanium dioxide composite powder, which provides antibacterial properties for the final glaze by loading silver ions.
[0015] A method for preparing sandstone glaze for the surface of ceramic ware comprises the following steps:
[0016] Mix the raw materials of various components according to the formula and add them into a grinding tank to form dry powder. Add 45-50% water by weight of the dry powder and grind for 10-12 hours. During the grinding process, the ratio of material, ball and water is controlled to be 1: (1-1.4): (0.4-0.6), preferably 1: 1.2: 0.5. After the grinding, a slurry is formed, which is deironed and sieved. The concentration is adjusted to a true specific gravity of 52-54 degrees, and then coated on the surface of ceramic utensils. After drying, it is sent to the kiln for oxidation firing. After natural cooling, it is taken out of the kiln to obtain sandstone glaze.
[0017] Beneficial effects of the present invention:
[0018] The invention prepares a sandstone glaze for the surface of ceramic ware, which uses potassium feldspar, kaolin, calcium carbonate and talcum powder as raw materials. The prepared glaze has a matte-like effect, and different metals can be added according to customer needs to form a special gloss appearance. The addition of quartz sand brings a rough feel to the glaze. In addition, the invention adds a composite powder. In the preparation process, urea is used as a precipitant, and silver ions and chloride ions are reacted to generate silver chloride precipitation through a combination of uniform precipitation and coprecipitation. The formed silver chloride is used as a crystal seed, and titanium oxysulfate is hydrolyzed under alkaline conditions to form titanium hydroxide deposited on the surface of the silver chloride crystal, and then phosphate ions are added to precipitate zirconium ions and titanium ions, and finally calcined to form a composite powder. The composite powder is a silver-loaded titanium dioxide composite powder, and antibacterial performance is provided for the final glaze by loading silver ions. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] A formula for a sandstone glaze for the surface of ceramic ware, comprising the following raw materials by weight: 20 parts of potassium feldspar, 3 parts of kaolin, 10 parts of calcium carbonate, 7 parts of talc, 5 parts of dolomite, 25 parts of quartz sand, 5 parts of barium carbonate, 2 parts of zirconium silicate, 1 part of aluminum oxide, and 5 parts of composite powder;
[0022] The surface of the ceramic ware is made of sandstone glaze comprising the following steps:
[0023] Mix the raw materials of various components according to the formula and add them into a grinding jar to form dry powder. Add 45% water by weight of the dry powder and grind for 10 hours. During the grinding process, the ratio of material, ball and water is controlled to be 1:1.2:0.5. After the grinding, a slurry is formed, which is deironed and sieved. The concentration is adjusted to a true specific gravity of 52 degrees. Then, it is coated on the surface of ceramic utensils. The coating thickness is controlled to be 1mm. After drying, it is sent to the kiln for oxidation firing. After natural cooling, it is taken out of the kiln to obtain sandstone glaze.
[0024] The oxidation sintering process is divided into three stages: the first stage: from room temperature to 650°C, with a controlled heating rate of 3°C / min; the second stage: from 650 to 850°C, with a controlled heating rate of 3.5°C / min; the third stage: from 850 to 1100°C, with a controlled heating rate of 2°C / min, and the highest temperature is kept for 15 minutes.
[0025] The composite powder is prepared by the following steps:
[0026] Step S1, adding urea to deionized water, stirring at a uniform speed and adding polyvinyl pyrrolidone, stirring at a uniform speed for 5 minutes, adding a 0.05 mol / L sodium chloride solution, stirring at a speed of 200 r / min for 5 minutes, adding a defoamer, slowly dropping a 0.05 mol / L silver nitrate solution while stirring, stirring at a uniform speed and reacting for 2 hours after the addition is completed, adding a 10% mass fraction of titanyl sulfate and a 15% mass fraction of zirconium sulfate solution to obtain a mixed solution, and controlling the amount ratio of urea, polyvinyl pyrrolidone, sodium chloride solution, defoamer, silver nitrate solution and deionized water to be 3g: 0.1g: 20mL: 0.05g: 20mL: 100mL;
[0027] Step S2, heating the mixed solution to 90°C, keeping the temperature for reaction for 4 hours, taking out and placing in an ice water bath to cool to room temperature after the reaction is completed, slowly dropping 8% by mass of disodium hydrogen phosphate aqueous solution, stirring at a uniform speed and reacting for 2 hours, vacuum filtering after the reaction is completed, washing the filter cake three times with deionized water and anhydrous ethanol in sequence, drying and calcining after washing to obtain an antibacterial powder, and controlling the amount of disodium hydrogen phosphate aqueous solution to be 8% by volume of the mixed solution.
[0028] Example 2
[0029] A formula for a sandstone glaze for the surface of ceramic ware, comprising the following raw materials by weight: 25 parts of potassium feldspar, 4 parts of kaolin, 11 parts of calcium carbonate, 8 parts of talc, 8 parts of dolomite, 35 parts of quartz sand, 6 parts of barium carbonate, 4 parts of zirconium silicate, 2.5 parts of aluminum oxide, and 8 parts of composite powder;
[0030] The surface of the ceramic ware is made of sandstone glaze comprising the following steps:
[0031] Mix the raw materials of various components according to the formula and add them into a grinding jar to form dry powder. Add 45-50% water by weight of the dry powder and grind for 10-12 hours. During the grinding process, the ratio of material, ball and water is controlled to be 1:1.2:0.5. After the grinding, a slurry is formed, which is sieved to remove iron and the concentration is adjusted to a true specific gravity of 53 degrees. It is then coated on the surface of ceramic utensils with a coating thickness of 2mm. After drying, it is sent to the kiln for oxidation firing and naturally cooled before being taken out of the kiln to obtain sandstone glaze.
[0032] The oxidation sintering process is divided into three stages: the first stage: from room temperature to 650°C, with a controlled heating rate of 3°C / min; the second stage: from 650 to 850°C, with a controlled heating rate of 3.5°C / min; the third stage: from 850 to 1100°C, with a controlled heating rate of 2°C / min, and the highest temperature is kept for 15 minutes.
[0033] The composite powder is prepared by the following steps:
[0034] Step S1, adding urea to deionized water, stirring at a uniform speed and adding polyvinyl pyrrolidone, stirring at a uniform speed for 5 minutes, adding a 0.05 mol / L sodium chloride solution, stirring at a speed of 200 r / min for 5 minutes, adding a defoamer, slowly dropping a 0.05 mol / L silver nitrate solution while stirring, stirring at a uniform speed and reacting for 2 hours after the addition is completed, adding a 10% mass fraction of titanyl sulfate and a 15% mass fraction of zirconium sulfate solution to obtain a mixed solution, and controlling the amount ratio of urea, polyvinyl pyrrolidone, sodium chloride solution, defoamer, silver nitrate solution and deionized water to be 4g:0.1g:22mL:0.06g:20mL:100mL;
[0035] Step S2, heating the mixed solution to 90°C, keeping the temperature for reaction for 4 hours, taking out and placing in an ice water bath to cool to room temperature after the reaction is completed, slowly dropping 8% sodium hydrogen phosphate aqueous solution by mass, stirring at a uniform speed and reacting for 2 hours, vacuum filtering after the reaction is completed, washing the filter cake three times with deionized water and anhydrous ethanol in sequence, drying and calcining after washing to obtain an antibacterial powder, and controlling the amount of sodium hydrogen phosphate aqueous solution to be 10% of the volume of the mixed solution.
[0036] Example 3
[0037] A formula for a sandstone glaze for the surface of ceramic ware, comprising the following raw materials by weight: 35 parts of potassium feldspar, 5 parts of kaolin, 12 parts of calcium carbonate, 10 parts of talc, 10 parts of dolomite, 50 parts of quartz sand, 8 parts of barium carbonate, 5 parts of zirconium silicate, 3.5 parts of aluminum oxide, and 10 parts of composite powder;
[0038] The surface of the ceramic ware is made of sandstone glaze comprising the following steps:
[0039] Mix the raw materials of various components according to the formula and add them into a grinding jar to form dry powder. Add 50% water by weight of the dry powder and grind for 12 hours. During the grinding process, the ratio of material, ball and water is controlled to be 1:1.2:0.5. After grinding, a slurry is formed, which is sieved to remove iron and the concentration is adjusted to a true specific gravity of 52-54 degrees. Then, it is coated on the surface of ceramic utensils with a coating thickness of 2.5mm. After drying, it is sent to the kiln for oxidation firing and naturally cooled. Then, it is taken out of the kiln to obtain sandstone glaze.
[0040] The oxidation sintering process is divided into three stages: the first stage: from room temperature to 650°C, with a controlled heating rate of 3°C / min; the second stage: from 650 to 850°C, with a controlled heating rate of 3.5°C / min; the third stage: from 850 to 1100°C, with a controlled heating rate of 2°C / min, and the highest temperature is kept for 15 minutes.
[0041] The composite powder is prepared by the following steps:
[0042] Step S1, adding urea to deionized water, stirring at a uniform speed and adding polyvinyl pyrrolidone, stirring at a uniform speed for 5 minutes, adding a 0.05 mol / L sodium chloride solution, stirring at a speed of 200 r / min for 5 minutes, adding a defoamer, slowly dropping a 0.05 mol / L silver nitrate solution while stirring, stirring at a uniform speed and reacting for 2 hours after the addition is completed, adding a 10% mass fraction of titanyl sulfate and a 15% mass fraction of zirconium sulfate solution to obtain a mixed solution, and controlling the amount ratio of urea, polyvinyl pyrrolidone, sodium chloride solution, defoamer, silver nitrate solution and deionized water to be 5g:0.2g:22mL:0.08g:20mL:100mL;
[0043] Step S2, heating the mixed solution to 90°C, keeping the temperature for reaction for 4 hours, taking out and placing in an ice water bath to cool to room temperature after the reaction is completed, slowly dropping 8% by mass of disodium hydrogen phosphate aqueous solution, stirring at a uniform speed and reacting for 2 hours, vacuum filtering after the reaction is completed, washing the filter cake three times with deionized water and anhydrous ethanol in sequence, drying and calcining after washing to obtain an antibacterial powder, and controlling the amount of disodium hydrogen phosphate aqueous solution to be 8-12% of the volume of the mixed solution.
[0044] Comparative Example 1
[0045] This comparative example is an antibacterial ceramic produced by a certain company on the market.
[0046] The antibacterial properties of the ceramic glazes prepared in Examples 1-3 and Comparative Example 1 were tested, and the results are shown in Table 1 below:
[0047] The experimental bacteria are Escherichia coli, Staphylococcus aureus and Candida albicans. Take the fresh culture (18h-24h) of the third generation nutrient agar medium slant of the strain, wash off the bacterial moss, shake and mix, dilute the bacterial solution to 105-106cfu / mL with sterile saline for use, take 3cm×3cm samples of the different ceramic products obtained above and put them into a 250mL conical flask, add 95mL PBS and 5mL bacterial solution respectively, fix the conical flask on an oscillating shaker, shake at 270rpm for 12h, take it out and rinse it with PBS three times, then put the rinsed ceramic sample into 50mL PBS, use ultrasonic vibration to rinse off the bacteria attached to the surface of the ceramic sample; finally, take 5mL of PBS solution containing surface-adherent bacteria and evenly spread it on the culture medium plate for observation and counting.
[0048] Table 1
[0049]
[0050]
[0051] It can be seen from Table 1 above that the glazes prepared in Examples 1-3 of the present invention can impart excellent antibacterial properties to vessels.
[0052] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0053] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A sandstone glaze for the surface of ceramic ware, characterized in that: The formula of the sandstone glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 5 parts of kaolin, 12 parts of calcium carbonate, 10 parts of talc, 10 parts of dolomite, 50 parts of quartz sand, 8 parts of barium carbonate, 5 parts of zirconium silicate, 3.5 parts of aluminum oxide, and 10 parts of composite powder; The composite powder is prepared by the following steps: Step S1, adding urea to deionized water, stirring at a uniform speed and adding polyvinyl pyrrolidone, stirring at a uniform speed for 5 minutes, adding a 0.05 mol / L sodium chloride solution, stirring at a speed of 200 r / min for 5 minutes, adding a defoamer, slowly dropping a 0.05 mol / L silver nitrate solution while stirring, stirring at a uniform speed and reacting for 2 hours after the addition is completed, adding a 10% mass fraction of titanyl sulfate and a 15% mass fraction of zirconium sulfate solution to obtain a mixed solution, and controlling the amount ratio of urea, polyvinyl pyrrolidone, sodium chloride solution, defoamer, silver nitrate solution and deionized water to be 5g:0.2g:22mL:0.08g:20mL:100mL; Step S2, heating the mixed solution to 90°C, keeping the temperature for reaction for 4 hours, taking out and placing in an ice water bath to cool to room temperature after the reaction, slowly dropping 8% sodium hydrogen phosphate aqueous solution, stirring at a uniform speed and reacting for 2 hours, vacuum filtering after the reaction, washing the filter cake three times with deionized water and anhydrous ethanol in sequence, drying and calcining after washing to obtain antibacterial powder, and controlling the amount of sodium hydrogen phosphate aqueous solution to be 8-12% of the volume of the mixed solution; The surface of the ceramic ware is made of sandstone glaze comprising the following steps: Mix the raw materials of each component according to the formula and add them into the grinding tank to form dry powder. Add 50% water by weight of the dry powder and grind for 12 hours. During the grinding process, the ratio of material, ball and water is controlled to be 1:1.2:0.
5. After the grinding, a slurry is formed, iron is removed and sieved, and the concentration is adjusted to a true specific gravity of 52-54 degrees. Then, it is coated on the surface of ceramic utensils with a coating thickness of 2.5mm. After drying, it is sent to the kiln for oxidation firing, and naturally cooled and discharged from the kiln to obtain sandstone glaze. The oxidation sintering process is divided into three stages: the first stage: from room temperature to 650°C, with a controlled heating rate of 3°C / min; the second stage: from 650 to 850°C, with a controlled heating rate of 3.5°C / min; the third stage: from 850 to 1100°C, with a controlled heating rate of 2°C / min, and the highest temperature is kept for 15 minutes.
2. The method for preparing a sandstone glaze for the surface of ceramic ware according to claim 1, characterized in that: The steps include: Mix the raw materials of various components according to the formula and add them into a grinding jar to form dry powder. Water is added and ground for 12 hours. During the grinding process, the ratio of material, balls and water is controlled to be 1:1.2:0.
5. After the grinding, a slurry is formed, which is sieved to remove iron and then coated on the surface of ceramic utensils. After drying, it is sent to the kiln for oxidation firing and naturally cooled before being taken out of the kiln to obtain sandstone glaze.
3. The method for preparing a sandstone glaze for the surface of ceramic ware according to claim 2, characterized in that: The amount of water used is 50% of the dry powder weight.
4. The method for preparing a sandstone glaze for the surface of ceramic ware according to claim 2, characterized in that: The concentration of the slurry is adjusted to a true specific gravity of 52-54 degrees.