A corrosion-resistant cast low-carbon steel material and preparation method thereof

CN116145039BActive Publication Date: 2024-10-29HUBEI TAIKE FRICTION MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310166668.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-10-29
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

Low carbon steel materials have poor corrosion resistance after casting, which limits their wide application. Traditional heat treatment increases cost and energy consumption. Existing technology smelting in a non-vacuum environment leads to an increase in impurities, which affects the quality of the profile.

Method used

Through alloying and post-casting treatment, combined with the corrosion inhibitor immersion treatment formulated with Lagerstroemia macrophylla extract, the corrosion resistance of low carbon steel is improved while retaining high strength. The specific steps include alloying treatment, post-casting heat treatment and corrosion inhibitor immersion. deal with.

Benefits of technology

The corrosion resistance of low carbon steel is significantly improved, with the yield strength reaching more than 800MPa. It also reduces the chemical corrosion process, extends the service life and improves the profile quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004096094090000071
    Figure BDA0004096094090000071
  • Figure BDA0004096094090000081
    Figure BDA0004096094090000081
Patent Text Reader

Abstract

The invention proposes a corrosion-resistant cast low-carbon steel material and a preparation method thereof. The materials include the following components in weight percentage: C0.07-0.24%, Mn0.26-0.87%, Si1.3-1.7%, P0.01-0.03%, S0.02-0.05%, Ni0.12-0.14%, Ti0.32-0.48% and B0.06-0.14%, and the balance is Fe. The method comprises the following steps: S1, melting Fe as a matrix, and performing desulfurization, deoxidation and alloying treatments; S2, performing casting and post-casting treatment; S3, and finally performing soaking treatment with a corrosion inhibitor. The corrosion-resistant cast low-carbon steel of the invention uses a combination of Mn, Si, Ni, Ti and B, is subjected to alloying and post-casting treatment to improve strength, and is subjected to corrosion inhibitor treatment prepared by a crape myrtle extract and acid to form an inhibition film on the surface, thereby preferably improving the corrosion resistance of the cast low-carbon steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material preparation, and in particular to a corrosion-resistant cast low-carbon steel material and a preparation method thereof. Background Art

[0002] Casting, as a basic process in the modern machinery manufacturing industry, can achieve high-efficiency and low-cost forming of complex metal workpieces. In the traditional casting process, heat treatment and plastic deformation are carried out after casting to improve the hardness and strength of cast steel. As an important material for the preparation of structural parts such as bolts, bearings and rivets, low-carbon steel has always been favored due to its excellent characteristics of low cost, high toughness and high plasticity. However, the more common low-carbon steel materials in the past had a yield strength of 200-400Mpa and a hardness of about 4GPa, and reprocessing would increase a lot of manpower and energy costs, which also limited the widespread application of low-carbon steel. On the other hand, low-carbon steel has excellent mechanical properties, but its corrosion resistance has no advantage over other materials. Poor corrosion resistance is a more prominent disadvantage of cast steel materials.

[0003] Steel corrosion is generally divided into chemical corrosion and electrochemical corrosion. The former is a chemical reaction between steel materials and oxidizing substances under dry or non-electrolyte solution conditions, while the latter is an oxidation-reduction reaction between steel materials and gases and liquids. Steel corrosion affects the surface quality of castings, profile wear, fatigue failure, and greatly reduces the service life, which hinders the application scope and technical development of cast low-carbon steel. Therefore, improving the corrosion resistance of low-carbon steel materials while maintaining basic yield strength is a technical problem that needs to be solved in this field.

[0004] CN105603297A discloses a method for preparing high-strength, corrosion-resistant low-carbon steel, which improves the corrosion resistance of low-carbon steel by using refining agents and controlling the post-casting heat treatment temperature. However, in this solution, the molten steel is smelted in a non-vacuum environment, and the oxygen content of the molten steel is too high, resulting in an increase in impurities in the low-carbon steel, which affects the quality of the profile. Summary of the invention

[0005] In view of this, the present invention proposes a corrosion-resistant cast low-carbon steel material and a preparation method thereof, which improves the corrosion resistance of the low-carbon steel while retaining good strength through alloying, post-casting and corrosion-inhibiting liquid treatment.

[0006] The technical solution of the present invention is achieved in this way:

[0007] On the one hand, the present invention provides a corrosion-resistant cast low-carbon steel material, which, based on the total weight percentage as 100%, includes the following components: C0.07-0.24%, Mn0.26-0.87%, Si1.3-1.7%, P0.01-0.03%, S0.02-0.05%, Ni0.12-0.14%, Ti0.32-0.48% and B0.06-0.14%, and the balance is Fe.

[0008] On the other hand, the present invention also provides a method for preparing a corrosion-resistant cast low-carbon steel material, comprising the following steps:

[0009] S1, melt Fe as a matrix, and perform desulfurization, deoxidation and alloying treatment;

[0010] S2, then casting and post-casting treatment;

[0011] S3. Finally, the steel is soaked in a corrosion-inhibiting liquid to obtain a corrosion-resistant cast low-carbon steel material.

[0012] On this basis, preferably, the order of components input into the alloying treatment in step S1 is 1) Si, Ni and B; 2) Ti; 3) remaining components.

[0013] On this basis, preferably, the temperature of the alloying treatment in step S1 is 1550-1750°C.

[0014] On this basis, preferably, the alloying process in step S1 includes the following steps: at 1550-1750°C, adding in the order of 1) Si, Ni and B; 2) Ti; 3) the remaining components, and performing alloying treatment by in-package injection method.

[0015] On this basis, preferably, the casting process in step S2 includes the following steps: after the alloying treatment in step S1, the temperature is lowered to 1300-1350° C. and casting is performed.

[0016] On this basis, preferably, the post-casting treatment in step S2 comprises the following steps:

[0017] A1. Heat to 900-950℃ for 4-5h, then reduce to 550-650℃ for 0.5-1.5h;

[0018] A2. Heat treatment at 300-350℃ for 2-4h, then heat treatment at 450-530℃ for 3-4h.

[0019] On this basis, preferably, the corrosion inhibition solution in step S3 comprises the following raw materials in parts by weight: 1-3 parts of Lagerstroemia indica extract and 9-12 parts of acid solution.

[0020] On this basis, preferably, the immersion treatment in step S3 comprises the following steps: immersing the low carbon steel obtained in step S2 in a corrosion inhibition solution at 20-25°C for 7-10 days.

[0021] On this basis, preferably, the preparation process of the Lagerstroemia indica extract comprises the following steps:

[0022] B1. Weigh the leaves of Lagerstroemia indica, dry them, grind them, add methanol and stir for 0.5-1h, extract them continuously at 40-45℃ for 4-5h to obtain an extract;

[0023] B2. Vacuum concentration and drying to obtain the Lagerstroemia indica extract.

[0024] On this basis, preferably, the acid solution is hydrochloric acid or nitric acid with a concentration of 1-1.5M.

[0025] On this basis, preferably, in step B1, the mass ratio of Lagerstroemia indica leaves to methanol is 1:(4.2-7.3).

[0026] Compared with the prior art, the corrosion-resistant cast low-carbon steel material and the preparation method thereof of the present invention have the following advantages:

[0027] Beneficial effects:

[0028] (1) The present invention uses a corrosion inhibition solution prepared by using Lagerstroemia indica and acid to immerse low-carbon steel. The Lagerstroemia indica extract forms an Fe-Lagerstroemia indica extract complex during the corrosion reaction process. At the same time, the active groups of the Lagerstroemia indica extract form an inhibitory film on the surface of the low-carbon steel, which effectively slows down the chemical corrosion process of the low-carbon steel and improves the corrosion resistance of the low-carbon steel.

[0029] (2) Although some of the current low-carbon steels for casting have improved corrosion resistance, their strength is still relatively poor. The present invention forms a low-carbon steel with high strength by setting the ratio of raw materials such as Ni, Ti and Mn, the reaction sequence, and the alloying and post-casting treatment processes, and the yield strength can reach more than 800 MPa. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A corrosion-resistant cast low-carbon steel material comprises the following components based on 100% by total weight: 0.07% C, 0.26% Mn, 1.3% Si, 0.01% P, 0.02% S, 0.12% Ni, 0.32% Ti and 0.06% B, with the balance being Fe.

[0033] The preparation process of the crape myrtle extract comprises the following steps:

[0034] B1. Weigh the leaves of Lagerstroemia indica, dry them, grind them, add methanol at a mass ratio of 1:4.2, stir for 0.5 h, and continuously extract at 40 °C for 4 h to obtain an extract;

[0035] B2. Vacuum concentration and drying to obtain the Lagerstroemia indica extract.

[0036] One part of the big-leaf crape myrtle extract and 9 parts of 1M hydrochloric acid were prepared into a corrosion inhibition solution.

[0037] A method for preparing a corrosion-resistant cast low-carbon steel material comprises the following steps:

[0038] S1. Fe is melted as a matrix and subjected to desulfurization and deoxidation treatment. At 1550°C, 1) Si, Ni and B; 2) Ti; 3) the remaining components are added in the order of 1) Si, Ni and B; 2) Ti; 3) the remaining components are added and alloyed by the in-package injection method;

[0039] S2. After alloying treatment in step S1, the temperature is lowered to 1300°C for casting. After casting, the temperature is first raised to 900°C for heat treatment for 4 hours, then lowered to 550°C for heat treatment for 0.5 hours, then lowered to 300°C for heat treatment for 2 hours, and then raised to 450°C for heat treatment for 3 hours.

[0040] S3. Finally, the low carbon steel obtained in step S2 is immersed in the corrosion inhibitor for 7 days at 20° C. to obtain a corrosion-resistant cast low carbon steel material.

[0041] Example 2

[0042] A corrosion-resistant cast low-carbon steel material comprises the following components based on 100% by total weight: 0.24% C, 0.87% Mn, 1.7% Si, 0.03% P, 0.05% S, 0.14% Ni, 0.48% Ti and 0.14% B, with the balance being Fe.

[0043] The preparation process of the crape myrtle extract comprises the following steps:

[0044] B1. Weigh the leaves of Lagerstroemia indica, dry them, grind them, add methanol at a mass ratio of 1:7.3, stir for 1 hour, and continuously extract at 45°C for 5 hours to obtain an extract;

[0045] B2. Vacuum concentration and drying to obtain the Lagerstroemia indica extract.

[0046] Three parts of the big-leaf crape myrtle extract and 12 parts of 1.5M hydrochloric acid were prepared into a corrosion inhibition solution.

[0047] A method for preparing a corrosion-resistant cast low-carbon steel material comprises the following steps:

[0048] S1. Fe is melted as a matrix and subjected to desulfurization and deoxidation treatment. At 1750°C, 1) Si, Ni and B; 2) Ti; 3) the remaining components are added in the order of 1) Si, Ni and B; 2) Ti; 3) the remaining components are added and alloyed by the in-package injection method;

[0049] S2. After alloying treatment in step S1, the temperature is lowered to 1350°C for casting. After casting, the temperature is first raised to 950°C for heat treatment for 5 hours, then lowered to 650°C for heat treatment for 1.5 hours, then lowered to 350°C for heat treatment for 4 hours, and then raised to 530°C for heat treatment for 4 hours.

[0050] S3. Finally, the low carbon steel obtained in step S2 is immersed in the corrosion inhibitor for 10 days at 25° C. to obtain a corrosion-resistant cast low carbon steel material.

[0051] Example 3

[0052] A corrosion-resistant cast low-carbon steel material comprises the following components based on 100% by total weight: 0.12% C, 0.57% Mn, 1.5% Si, 0.02% P, 0.03% S, 0.13% Ni, 0.40% Ti and 0.10% B, with the balance being Fe.

[0053] The preparation process of the crape myrtle extract comprises the following steps:

[0054] B1. Weigh the leaves of Lagerstroemia indica, dry them, grind them, add methanol at a mass ratio of 1:5.5, stir for 0.6 h, and continuously extract at 42 °C for 4.2 h to obtain an extract;

[0055] B2. Vacuum concentration and drying to obtain the Lagerstroemia indica extract.

[0056] 2 parts of Lagerstroemia indica extract and 10 parts of nitric acid with a molar concentration of 1M were prepared into a corrosion inhibition solution.

[0057] A method for preparing a corrosion-resistant cast low-carbon steel material comprises the following steps:

[0058] S1. Fe is melted as a matrix and subjected to desulfurization and deoxidation treatment. At 1650°C, 1) Si, Ni and B; 2) Ti; 3) the remaining components are added in the order of 1) Si, Ni and B; 2) Ti; 3) the remaining components are added and alloyed by the in-package injection method;

[0059] S2. After alloying treatment in step S1, the temperature is lowered to 1330°C for casting. After casting, the temperature is first raised to 940°C for heat treatment for 4.5 hours, then lowered to 600°C for heat treatment for 1 hour, lowered to 320°C for heat treatment for 3 hours, and then raised to 500°C for heat treatment for 3.5 hours.

[0060] S3. Finally, the low carbon steel obtained in step S2 is immersed in the corrosion inhibitor for 8 days at 22° C. to obtain a corrosion-resistant cast low carbon steel material.

[0061] Comparative Example 1

[0062] A cast low-carbon steel material, which differs from Example 1 in that it comprises the following components: C0.24%, Mn0.87%, Si1.7%, P0.03%, S0.05%, Ni0.14% and Co1.3%, with the balance being Fe, and no alloying or post-casting treatment is performed.

[0063] Comparative Example 2

[0064] A cast low-carbon steel material, which differs from Example 1 in that no corrosion-inhibiting liquid immersion treatment is used.

[0065] Comparative Example 3

[0066] A cast low-carbon steel material, with reference to the patent preparation process with publication number CN105603297A.

[0067] Performance Testing

[0068] The cast low-carbon steel obtained in Examples 1-3 and Comparative Examples 1-3 was cut into 15 mm × 15 mm, 2.5 mm thick samples, and the corrosion resistance was tested by electrochemical impedance spectroscopy (EIS). A 5% sodium chloride solution was used as the corrosion solution, the test temperature was 25°C, the auxiliary electrode was a 2 mm platinum disk electrode, the reference electrode was a silver chloride / silver electrode, the scanning rate was 0.01 v / s, the scanning potential was ±0.5 v, the standing time was 2 min, the corrosion potential and corrosion current density of the samples were tested, the test was repeated three times, and the average was taken; in addition, the mechanical properties of the low-carbon steel were tested to test its yield strength and tensile strength.

[0069] Table 1 Corrosion resistance test of low carbon steel in Examples 1-3 and Comparative Examples 1-3

[0070] Example Corrosion potential / v <![CDATA[Corrosion current density / 10 -5 A·cm -2 > Example 1 -0.620 0.394 Example 2 -0.607 0.435 Example 3 -0.592 0.574 Comparative Example 1 -0.435 0.808 Comparative Example 2 -0.394 0.912 Comparative Example 3 -0.562 0.477

[0071] Table 2 Mechanical properties test of low carbon steel of Examples 1-3 and Comparative Examples 1-3

[0072]

[0073]

[0074] It can be seen from the above that the cast low-carbon steel material of the present invention has a high corrosion potential, a low corrosion current density, and excellent corrosion resistance, while the mechanical properties also maintain a certain strength.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A corrosion-resistant cast low-carbon steel material, It is characterized in that Based on the total weight percentage of 100%, it is composed of the following components: C 0.07-0.24%, Mn 0.26-0.87%, Si 1.3-1.7%, P 0.01-0.03%, S 0.02-0.05%, Ni 0.12-0.14%, Ti 0.32-0.48% and B 0.06-0.14%, and the balance is Fe; The method for preparing the corrosion-resistant cast low-carbon steel material comprises the following steps: S1, melt Fe as a matrix, and perform desulfurization, deoxidation and alloying treatment; S2, then casting and post-casting treatment; S3. Finally, the corrosion-resistant casting low-carbon steel material is obtained by soaking in a corrosion-inhibiting liquid; The corrosion inhibition solution in step S3 comprises the following raw materials in parts by weight: 1-3 parts of Lagerstroemia indica extract and 9-12 parts of acid solution; the acid solution is hydrochloric acid or nitric acid, and the molar concentration is 1-1.5M; The immersion treatment in step S3 comprises the following steps: immersing the low carbon steel obtained in step S2 in a corrosion inhibition solution at 20-25° C. for 7-10 days; The preparation process of the Lagerstroemia indica extract comprises the following steps: B1. Weigh the leaves of Lagerstroemia indica, dry them, grind them, add methanol and stir for 0.5-1h, extract them continuously at 40-45℃ for 4-5h to obtain an extract; B2. Vacuum concentration and drying to obtain the Lagerstroemia indica extract.

2. The method for preparing the corrosion-resistant cast low-carbon steel material according to claim 1, It is characterized in that The order of components added in the alloying treatment in step S1 is 1) Si, Ni and B; 2) Ti; 3) remaining components.

3. The method for preparing the corrosion-resistant cast low-carbon steel material according to claim 1, It is characterized in that The temperature of the alloying treatment in step S1 is 1550-1750°C.

4. The method for preparing the corrosion-resistant cast low-carbon steel material according to claim 1, It is characterized in that The post-casting treatment in step S2 comprises the following steps: A1. Heat to 900-950℃ for 4-5h, then reduce to 550-650℃ for 0.5-1.5h; A2. Heat treatment at 300-350℃ for 2-4h, then heat treatment at 450-530℃ for 3-4h.

5. The method for preparing the corrosion-resistant cast low-carbon steel material according to claim 1, It is characterized in that In step B1, the mass ratio of Lagerstroemia indica leaves to methanol is 1:(4.2-7.3).

Citation Information

Patent Citations

  • Preparation method of high-strength and corrosion-resistant low-carbon steel

    CN105603297A

  • Metal polishing solution and metal polishing method

    CN113403622A

  • Steel sheet for hot press having excellent hot workability, and automotive member

    JP2005126733A