Ethylene resin composition and molded article

By preparing a mixture of high-density and low-density polyethylene within a specific density range, the problem of insufficient morphological stability and strength retention of vinyl resin compositions at high temperatures is solved, and the effects of reducing fish eyes and excellent heat resistance are achieved. Meets the requirements of economy and high temperature performance.

CN116162299BActive Publication Date: 2024-10-22ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211487714.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-11-25
Publication Date
2024-10-22
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

It is difficult for existing vinyl resin compositions to maintain morphological stability and strength under high temperature conditions. At the same time, there is a problem of reduced fish eyes (FE), and there is a trade-off between economic efficiency and excellent heat resistance.

Method used

By preparing a mixture of high-density polyethylene and low-density polyethylene with a density of 920kg/m3 or more and 945kg/m3 or less, satisfying specific melt flow rate, density, dynamic viscoelasticity and melting peak characteristics, combined with preferred polymerization conditions and The manufacturing method forms a vinyl resin composition having excellent heat resistance, morphological stability and blocking resistance.

Benefits of technology

A vinyl resin composition with excellent morphological stability and strength retention at high temperatures, good adhesion resistance, and effective reduction of fisheyes has been realized, which combines economy and high-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116162299B_ABST
    Figure CN116162299B_ABST
Patent Text Reader

Abstract

The present invention relates to an ethylene resin composition and a molded body. The present invention provides an ethylene resin composition that has excellent morphological stability at high temperatures and strength retention at high temperatures, excellent blocking resistance, and reduced fish eyes. An ethylene resin composition that satisfies <Condition (A)> to <Condition (D)>. <Condition (A)> The melt flow rate at 190°C and a load of 2.16 kg is greater than 1.0 g / 10 minutes and less than 20.0 g / 10 minutes. <Condition (B)> The density is 920 kg / m 3 Above and 945kg / m 3 <Condition (C)> In the ARES temperature measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 115°C to 145°C. <Condition (D)> In the ARES temperature measurement, the value of tan δ at 150°C is 1.00 to 1.50.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an ethylene resin composition and a molded article. Background Art

[0002] Ethylene resin compositions are molded by various molding methods and used in a variety of applications. Different properties are required depending on the molding methods and applications.

[0003] As a representative application of the ethylene resin composition, films can be cited. Specifically, surface protective films for optical components and the like are known. For the purpose of preventing damage and stains from the outside during processing, transportation, and storage, the surface protective films are pasted on the surfaces of adherends such as metal plates, resin plates, wooden decorative plates, nameplates, liquid crystal components, electrical and electronic components, building materials, and automobile parts.

[0004] The ethylene resin composition used for the surface protection film is required to have few fish eyes (hereinafter also referred to as "FE") in order not to damage the substrate to be protected. It should be noted that the above-mentioned FE refers to the small spherical foreign matter and defect structure existing in the film made by using the above-mentioned ethylene resin composition.

[0005] As representative methods for producing such FE-less ethylene resin compositions, for example, a method of removing using a sintered filter and a method of mixing high-density polyethylene and low-density polyethylene are known (see, for example, Patent Documents 1 to 2).

[0006] As mentioned above, the adherend of the object protected by the surface film is sometimes processed under the state of being pasted with the surface protection film. For example, in the case of protecting the adherend exposed to high temperature in the processes such as the drying process and the molding process, it is required to have a high heat resistance that will not cause shrinkage or curling due to heat and to have morphological stability and strength so that the surface protection film of the adherend can be protected at high temperatures even at high temperatures. In addition, the surface protection film is usually manufactured by sending out from a roller, therefore, in the case of using the ethylene resin composition for the outer layer of the surface protection film, it is important to easily send out from a roller.

[0007] From the above viewpoints, an ethylene resin composition having excellent heat resistance, morphological stability at high temperatures, and blocking resistance and having appropriate flexibility is required.

[0008] As a method for obtaining a surface protective film with high heat resistance and excellent anti-blocking and flexibility, a method of mixing crystalline polypropylene polymers and elastomers in ethylene resins is disclosed (for example, with reference to patent document 3). This method is not preferred from the perspective of economics and reuse, and has the problem that there is still room for improvement in the morphological stability and strength maintained at high temperatures. In addition, in patent document 3, FE is not verified. In addition, from the perspective of economics, it is required to use a separate ethylene resin composition to meet the characteristics of morphological stability and strength that can be maintained at high temperatures without mixing crystalline polypropylene polymers and elastomers, but in recent years, it is gradually further required that the ethylene resin composition has excellent heat resistance and excellent flexibility under high temperature conditions. However, usually heat resistance and flexibility are in a trade-off relationship, and the technology recorded in patent document 3 has the problem of not yet reaching improvement.

[0009] In addition, as a method for obtaining an ethylene resin composition having excellent heat resistance and transparency, a method of mixing high-density polyethylene and low-density polyethylene is disclosed (for example, refer to Patent Document 4). However, Patent Document 4 verifies that the high-temperature condition for heat resistance is around 120°C, and there is still room for improvement in terms of heat resistance at temperatures above 120°C, morphological stability at high temperatures, maintenance of strength at high temperatures, and reduction of FE.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent No. 4426441

[0013] Patent Document 2: Japanese Patent No. 6792957

[0014] Patent Document 3: Japanese Patent No. 6593168

[0015] Patent Document 4: Japanese Patent Application Publication No. 2018-44122 Summary of the invention

[0016] Problems to be solved by the invention

[0017] As described above, there has been a demand for an ethylene resin composition which has excellent morphological stability at high temperatures, retention of strength at high temperatures, and blocking resistance, and which achieves a reduction in FE.

[0018] Therefore, in view of the above-mentioned problems of the prior art, an object of the present invention is to provide an ethylene resin composition which is excellent in morphological stability at high temperatures, strength retention at high temperatures, and blocking resistance, and which achieves a reduction in FE.

[0019] Means used to solve problems

[0020] The present inventors have conducted intensive studies to solve the problems of the above-mentioned prior art and have found that an ethylene resin composition having the composition shown below and having specific properties can solve the problems of the above-mentioned prior art, thereby completing the present invention.

[0021] That is, the present invention is as follows. [1]

[0023] An ethylene-based resin composition, wherein the ethylene-based resin composition satisfies the following <Condition (A)> to <Condition (D)>.

[0024] <Condition (A)>

[0025] The ethylene resin composition has a melt flow rate of 1.0 g / 10 min or more and 20.0 g / 10 min or less under the conditions of 190° C. and a load of 2.16 kg.

[0026] <Condition (B)>

[0027] The density of the ethylene resin composition is 920 kg / m 3 Above and 945kg / m 3 the following.

[0028] <Condition (C)>

[0029] In the ARES temperature rise measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 115°C to 145°C.

[0030] <Condition (D)>

[0031] In the ARES temperature rise measurement, the value of tan δ at 150° C. is 1.00 or more and 1.50 or less. [2]

[0033] The ethylene resin composition as described in the above-mentioned [1], wherein

[0034] When the temperature is 170℃ and the shear rate is 10s -1 The melt viscosity of the ethylene resin composition measured under the conditions of

[0035] At 230°C and a shear rate of 10 s -1 When the melt viscosity of the ethylene resin composition measured under the conditions of is denoted as Y (Pa·s),

[0036] Satisfies the following formula (1):

[0037] 5≤(YX) / (170-230)≤25……(1). [3]

[0039] The ethylene resin composition as described in [1] or [2] above, wherein

[0040] In the temperature-heat flow curve of the ethylene resin composition obtained by differential scanning calorimetry (DSC), there are two or more melting peaks, the melting peak temperature on the highest temperature side is 118° C. or more, and

[0041] The difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is 10° C. or more and 30° C. or less. [4]

[0043] The ethylene resin composition as described in any one of [1] to [3] above, wherein the ethylene resin composition has a density of 942 kg / m 3 The above high-density polyethylene has a density of 930kg / m 3 A mixture of the following low density polyethylene. [5]

[0045] The ethylene resin composition as described in any one of [1] to [4] above, wherein the ethylene resin composition contains 10% by mass or more and 50% by mass or less of a compound having a density of 942 kg / m 3 High density polyethylene above. [6]

[0047] A molded article, wherein the molded article is a molded article of the ethylene resin composition according to any one of [1] to [5] above. [7]

[0049] The molded article according to the above-mentioned [6], wherein the molded article is a film.

[0050] Effects of the Invention

[0051] According to the present invention, it is possible to provide an ethylene-based resin composition which is excellent in morphological stability at high temperatures, in strength retention at high temperatures, and in blocking resistance, and in which FE is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 A state diagram showing an example of the relationship between the maximum value M, the minimum value m, and the average value (M+m) / 2 of tan δ in the temperature range of 30° C. to 150° C. in the ARES heating measurement of the ethylene resin composition. DETAILED DESCRIPTION

[0053] Hereinafter, a mode for carrying out the invention of the present application (hereinafter referred to as “the present embodiment”) will be described in detail.

[0054] It should be noted that the following embodiments are examples for explaining the present invention and are not intended to limit the present invention to the following contents. The present invention can be implemented with various modifications within the scope of the gist of the invention.

[0055] [Ethylene resin composition]

[0056] The ethylene resin composition of the present embodiment satisfies the following <Condition (A)> to <Condition (D)>.

[0057] <Condition (A)>

[0058] The ethylene resin composition has a melt flow rate of 1.0 g / 10 min or more and 20.0 g / 10 min or less under the conditions of 190° C. and a load of 2.16 kg.

[0059] <Condition (B)>

[0060] The density of the ethylene resin composition is 920 kg / m 3 Above and 945kg / m 3 the following.

[0061] <Condition (C)>

[0062] In the ARES temperature rise measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 115°C to 145°C.

[0063] <Condition (D)>

[0064] In the ARES temperature rise measurement, the value of tan δ at 150° C. is 1.00 or more and 1.50 or less.

[0065] By having the above-mentioned configuration, it is possible to obtain an ethylene-based resin composition which is excellent in morphological stability at high temperatures and strength retention at high temperatures, and is excellent in blocking resistance, and which achieves a reduction in FE.

[0066] The ethylene resin composition of this embodiment preferably further satisfies the following <Condition (E)> to <Condition (G)>. Thus, an ethylene resin composition having excellent morphological stability at high temperatures, excellent strength retention at high temperatures, excellent blocking resistance, and reduced FE can be obtained.

[0067] <Condition (E)>

[0068] When the temperature is 170℃ and the shear rate is 10s -1 The melt viscosity of the ethylene resin composition measured under the conditions of is set to X (Pa·s), and the temperature is set at 230°C and a shear rate of 10 s -1 When the melt viscosity of the ethylene resin composition measured under the conditions of is denoted as Y (Pa·s), the following formula (1) is satisfied.

[0069] 5≤(YX) / (170-230)≤25……Formula (1)

[0070] <Condition (F)>

[0071] In the temperature-heat flow curve of the ethylene resin composition obtained by differential scanning calorimetry (DSC), there are two or more melting peaks, the melting peak temperature on the highest temperature side is above 118°C, and the difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is above 10°C and below 30°C.

[0072] <Condition(G)>

[0073] The ethylene resin composition contains 10 mass % or more and 50 mass % or less of a 3 High density polyethylene above.

[0074] The content of high-density polyethylene is more preferably 15% to 45% by mass, and further preferably 20% to 40% by mass. Thus, an ethylene resin composition having excellent morphological stability at high temperatures, excellent strength retention at high temperatures, excellent blocking resistance, and reduced FE can be obtained.

[0075] The ethylene resin composition of this embodiment contains polyethylene, and preferably has a density of 942 kg / m 3 The above high-density polyethylene has a density of 930kg / m 3 The present invention also can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention. The present invention can be used for the preparation of the present invention.

[0076] The polyethylene contained in the ethylene-based resin composition of the present embodiment may be an ethylene homopolymer or a copolymer of ethylene and an α-olefin.

[0077] The method for producing polyethylene is not particularly limited, and polyethylene may be produced by any of the commonly used production methods of a solution method, a high-pressure method, a high-pressure bulk method, a gas method, or a slurry method.

[0078] (Melt flow rate (MFR) at 190°C and a load of 2.16 kg)

[0079] As shown in the above <Condition (A)>, the MFR of the ethylene resin composition of the present embodiment under the conditions of 190°C and a load of 2.16 kg is 1.0 g / 10 min or more and 20.0 g / 10 min or less, preferably 2.0 g / 10 min or more and 15.0 g / 10 min or less, and more preferably 3.0 g / 10 min or more and 10.0 g / 10 min or less.

[0080] When the MFR of the ethylene resin composition is 1.0 g / 10 minutes or more, the drape property of the film is improved and film breakage can be suppressed, which is preferred.

[0081] In addition, when the MFR of the ethylene resin composition is 20.0 g / 10 minutes or less, sufficient blocking resistance can be obtained and the morphological stability at high temperatures is excellent, which is preferred.

[0082] The MFR of the ethylene resin composition can be controlled by adjusting the polymerization conditions of polyethylene. Specifically, the MFR of the ethylene resin composition can be controlled within the above numerical range by adjusting the selection of the types of raw materials and the mixing ratio.

[0083] (density)

[0084] The density of the ethylene resin composition of this embodiment is 920 kg / m 3 Above and 945kg / m 3 Below. Preferably 928kg / m 3 Above 943kg / m 3 Below, more preferably 930kg / m 3 Above and 940kg / m 3 the following.

[0085] The density of the ethylene resin composition is 920 kg / m 3 The above mentioned film has improved heat resistance, so it is preferred. In addition, the density of the ethylene resin composition is 945 kg / m 3 Below this value is preferred because appropriate flexibility can be obtained.

[0086] In addition, the density of the ethylene-based resin composition is measured in accordance with JIS K7112, and is specifically measured by the method described in the examples described later.

[0087] The density of the ethylene resin composition can be controlled by adjusting the polymerization conditions of polyethylene. Specifically, the density of the ethylene resin composition can be controlled within the above numerical range by adjusting the selection of the types of raw materials and the mixing ratio.

[0088] (ARES temperature rise measurement)

[0089] For the ethylene resin composition of the present embodiment, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached in the ARES temperature rise measurement is 115°C to 145°C.

[0090] In the ARES temperature measurement, the dynamic viscoelasticity is measured while the sample is heated, so that the melting behavior of the sample and the viscoelasticity in a high temperature state can be analyzed. For example, the measurement can be performed by the following method.

[0091] Using ARES-G2 manufactured by TA Instruments, the gap distance was adjusted to 1mm to 2mm in a nitrogen atmosphere, and the storage modulus (G') and loss modulus (G") were measured using parallel plates with a diameter of 8mmφ, and their ratio G" / G' was taken as tanδ. The ethylene resin composition of the present embodiment is completely melted by heating the ethylene resin composition particles in an apparatus set to 200°C for 30 minutes. Then, the temperature is lowered from 200°C to 30°C at a rate of 5°C / min. When cooling, the distance between the plates is adjusted so that the normal stress is zero, taking into account the shrinkage of the sample and the fixture due to thermal expansion. Next, the dynamic viscoelasticity is measured while the temperature is raised from 30°C to 150°C at a rate of 5°C / min. As the temperature is raised, the strain amount changes between 0.1% and 5.0% according to the softening of the resin, and the measurement is performed. The strain is measured starting from 0.1% and changes according to the softening of the resin.

[0092] (Temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tanδ is reached)

[0093] For the ethylene resin composition of the present embodiment, in the ARES temperature rise measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 115°C to 145°C, preferably 118°C to 140°C, and more preferably 120°C to 135°C.

[0094] Here, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ is reached represents the temperature at which the viscoelasticity of the ethylene resin composition changes viscously due to melting. Figure 12 is a state diagram showing an example of the maximum value M, the minimum value m, and the average value (M+m) / 2 of tan δ in the temperature range of 30° C. to 150° C. in the ARES heating measurement of the ethylene resin composition.

[0095] When the temperature to reach (M+m) / 2 is 115°C or higher, excellent heat resistance is obtained, which is preferred. When the temperature to reach (M+m) / 2 is 145°C or lower, flexibility derived from the low-density component is obtained, which is preferred.

[0096] The temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tanδ is reached can be controlled within the above numerical range by adjusting the polymerization method, composition, and mixing method of the components contained in the ethylene resin composition. There is no particular limitation on the method, for example, by containing 10% by mass or more of high-density polyethylene having a melting point of 118°C or more in low-density polyethylene, the heat resistance of the ethylene resin composition is improved, and the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tanδ is reached can be adjusted to 115°C or more.

[0097] In addition, for example, by including less than 50 mass % of high-density polyethylene with a melting point of 118°C or above in low-density polyethylene or by not using ultra-high molecular weight components such as ultra-high molecular weight polyethylene with a weight average molecular weight of more than 1 million g / mol, the temperature reaching (M+m) / 2 can be adjusted to below 145°C.

[0098] On the other hand, high-density polyethylene and low-density polyethylene with large melting point differences are usually incompatible. When high-density polyethylene is not fully dispersed, due to the melting of low-density polyethylene as a matrix, the temperature having the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ becomes the tendency of the low temperature side.

[0099] By fully dispersing the high-density polyethylene in the low-density polyethylene, the temperature at which (M+m) / 2 is achieved is 115° C. or higher, and the heat resistance of the ethylene-based resin composition tends to be improved. The reason for this is that by fully dispersing the high-density polyethylene in the low-density polyethylene at the molecular level, the orientation relaxation and molecular movement of the low-density polyethylene are inhibited.

[0100] As a method for making low-density polyethylene and high-density polyethylene fully disperse and mix, there is no particular restriction, preferably two kinds of particles are fully dry mixed with each other, and then a method for melt blending is performed using a single screw extruder. In addition, by appropriately changing the rotating speed of the extruder, and controlling the variation of the resin pressure within 5MPa, high-density polyethylene and low-density polyethylene are easily and uniformly dispersed, so it is preferred. In addition, in the process of granulating the polymerized powder in the slurry polymerization process of high-density polyethylene, by premixing about 5% by mass of low-density polyethylene as an additive, in the mixing process of high-density polyethylene and low-density polyethylene thereafter, the compatibility of high-density polyethylene with low-density polyethylene is improved, so it is preferred. In addition, by adjusting the composition of the liquid co-catalyst component used during the polymerization of high-density polyethylene, the active state of the Ziegler-Natta catalyst is controlled, and a trace of high-molecular-weight components and low-molecular-weight components are generated in high-density polyethylene, so as to improve the compatibility with low-density polyethylene, so it is preferred.

[0101] (tanδ value at 150°C)

[0102] The ethylene resin composition of the present embodiment has a tan δ value of 1.00 to 1.50 at 150° C. in ARES temperature measurement, preferably 1.05 to 1.40, and more preferably 1.10 to 1.30.

[0103] Here, the tan δ value of the ethylene resin composition at 150° C. indicates the viscoelasticity in a molten state at a temperature not lower than the melting point. According to the definition of tan δ, a smaller tan δ value indicates greater elasticity.

[0104] When the value of tan δ is 1.00 or more, the film has a certain degree of fluidity, so it can be formed into a film using a T-die, which is preferred. In addition, when the value of tan δ is 1.50 or less, it has sufficient elasticity even in a molten state, and has excellent morphological stability and strength at high temperatures, which is preferred. In addition, it has sufficient elasticity during kneading in an extruder, so that FE derived from unmelted resin is dispersed, which is preferred.

[0105] The value of tan δ of the ethylene resin composition at 150°C can be controlled within the above numerical range by adjusting the polymerization method, composition, and mixing method of the components contained in the ethylene resin composition. As its method, for example, a method containing 50% by mass or more of a low-density polyethylene with a large number of long chain branches can be cited. Thus, by the entanglement of molecular chains with each other, even in a molten state, a certain degree of elasticity is maintained, and the value of tan δ at 150°C tends to be more than 1.00 and less than 1.50. As a method for manufacturing an ethylene resin composition containing 50% by mass or more of a low-density polyethylene with a large number of long chain branches, there is no particular limitation, and for example, a method for regulating the polymerization temperature, polymerization pressure, type of polymerization initiator or chain transfer agent, type of polymerization reactor, and the temperature of the ethylene gas supplied to the polymerization reactor can be cited. For example, by heating the pipeline immediately before the polymerization reactor with water vapor or the like, the ethylene gas is adjusted to about 150° C., and polymerization is carried out under forced stirring, whereby the entire polymerization reactor becomes nearly homogeneous, thereby tending to produce a polymer having a large number of branching points and obtain an ethylene resin composition containing 50% by mass or more of a low-density polyethylene having a large number of long-chain branches.

[0106] (Melt viscosity at 170°C and 230°C)

[0107] The ethylene resin composition of this embodiment is heated at 170°C and a shear rate of 10 s -1 The melt viscosity measured under the conditions of is set to X (Pa·s), and the temperature is 230°C and the shear rate is 10s -1 When the melt viscosity measured under the conditions of is defined as Y (Pa·s), (YX) / (170-230) is preferably 5 or more and 25 or less. It is more preferably 7 or more and 22 or less, and further preferably 10 or more and 20 or less.

[0108] (YX) / (170-230) represents the degree of change in melt viscosity with respect to temperature change.

[0109] When the value of the above formula is 5 or more, the film-forming property and processability in the temperature range of 170° C. to 230° C. are excellent, which is preferred. In addition, when the value of the above formula is 25 or less, the melt viscosity is not easily reduced with respect to temperature changes, and the morphological stability at high temperatures is excellent, which is preferred.

[0110] (YX) / (170-230) can be controlled by adjusting the branched structure of polyethylene contained in the ethylene resin composition. Examples of methods for adjusting the branched structure of polyethylene include methods of adjusting polymerization conditions such as polymerization temperature, polymerization pressure, and the type of polymerization initiator.

[0111] In addition, in order to manufacture an ethylene resin composition in which the value of (YX) / (170-230) is controlled within the range of 5 to 25, it is effective to more precisely control the branched structure of the low-density polyethylene. As a method thereof, for example, a method of adjusting the type of polymerization reactor and the temperature of the ethylene gas supplied to the polymerization reactor is effective. By heating the pipeline immediately before the polymerization reactor with water vapor or the like, the ethylene gas is adjusted to about 150°C, and polymerization is carried out under forced stirring, whereby the entire polymerization reactor becomes close to a homogeneous state, and it is easy to generate polyethylene with a large number of branching points. By using the low-density polyethylene obtained by polymerization in this way as a raw material, the decrease in melt viscosity under temperature changes becomes smaller, so it is preferred. That is, by adjusting the content of polyethylene with a large number of branching points, the degree of decrease in melt viscosity under temperature changes can be controlled, and the value of (YX) / (170-230) can be controlled within the numerical range of 5 to 25 as described above.

[0112] The melt viscosity of the ethylene resin composition can be measured by the method described in Examples below.

[0113] (Temperature-heat flow curve obtained by differential scanning calorimetry (DSC))

[0114] The ethylene resin composition of the present embodiment has two or more melting peaks in a temperature-heat flow curve (hereinafter also referred to as a "DSC curve") obtained by differential scanning calorimetry (DSC), the melting peak temperature on the highest temperature side is 118° C. or higher, and the difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is preferably 10° C. or higher and 30° C. or lower, more preferably 12° C. or higher and 28° C. or lower, and even more preferably 15° C. or higher and 25° C. or lower.

[0115] The observation of two or more melting peaks indicates that high-density polyethylene and low-density polyethylene are contained.

[0116] As a method for obtaining the above-mentioned ethylene resin composition, for example, a method of mixing high-density polyethylene with low-density polyethylene can be cited. In particular, by mixing high-density polyethylene with a melting point of 118°C or more and low-density polyethylene with a melting point of 108°C or less, an ethylene resin composition having a melting peak temperature of 118°C or more on the highest temperature side and a difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side of 10°C or more and 30°C or less can be obtained.

[0117] The difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is 10°C or more, because an ethylene resin composition and a film having both the heat resistance brought by the high-density polyethylene and the flexibility brought by the low-density polyethylene can be obtained, so it is preferred. The difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is 30°C or less, because the high-density polyethylene and the low-density polyethylene are in a state of moderate mixing, so it is preferred.

[0118] The measurement by DSC was carried out by the method described in Examples.

[0119] [Molding body]

[0120] The molded article of the present embodiment is a molded article of the ethylene resin composition of the present embodiment, and an example thereof is a film. When the film is a multilayer film, the ethylene resin composition of the present embodiment can be used for both the outermost layer and the intermediate layer.

[0121] [Method for producing ethylene resin composition]

[0122] The ethylene resin composition of the present embodiment can be produced, for example, by melt-kneading a high-density polyethylene (A) and a low-density polyethylene (B), but is not particularly limited.

[0123] As the melt-kneading machine in the mixing operation, for example, single screw extruder, twin screw extruder, exhaust extruder, tandem extruder etc. can be used. Particularly in order to improve the dispersibility of high density polyethylene and low density polyethylene, preferably particles are fully dry-mixed each other, and then single screw extruder is utilized to carry out melt-kneading. In addition, in order to suppress the uneven mixing of high density polyethylene and low density polyethylene, the rotating speed of the extruder is preferably appropriately changed, and the variation of resin pressure is controlled within 5MPa.

[0124] (Method for producing high-density polyethylene)

[0125] The high-density polyethylene (A) can be produced, for example, by a continuous slurry polymerization method.

[0126] The catalyst used in the manufacture is not particularly limited, and examples thereof include metallocene catalysts, Ziegler-Natta catalysts, Phillips catalysts, etc. By using a Ziegler-Natta catalyst having multiple active sites, the molecular weight distribution becomes broadened, and the compatibility with low-density polyethylene is improved, so it is preferred. In addition, usually, the physical properties of high-density polyethylene (A) can be controlled by adjusting the comonomer concentration, hydrogen concentration, and the type of cocatalyst in addition to adjusting the polymerization temperature, polymerization pressure, and catalyst type.

[0127] When the high-density polyethylene (A) and the low-density polyethylene (B) described later are copolymers of ethylene and other comonomers, examples of the comonomers include compounds selected from the group consisting of propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, vinylcyclohexane, styrene, and derivatives thereof. a cyclic olefin having 3 to 20 carbon atoms selected from the group consisting of cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene and 2-methyl-1,4,5,8-dimethylene-1,2,3,4,4a,5,8,8a-octahydronaphthalene; a linear, branched or cyclic diene having 4 to 20 carbon atoms selected from the group consisting of 1,3-butadiene, 1,4-pentadiene, 1,5-hexadiene, 1,4-hexadiene, 1,7-octadiene and cyclohexadiene, but not limited thereto. In the present embodiment, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene and 1-eicosene are particularly preferred.

[0128] The polymerization temperature of the high-density polyethylene (A) is preferably 30° C. to 100° C. A polymerization temperature of 30° C. or higher enables industrially more efficient production, while a polymerization temperature of 100° C. or lower enables continuous and more stable operation.

[0129] The polymerization pressure of the high-density polyethylene (A) is usually preferably normal pressure or higher and 2 MPa or lower, more preferably 0.1 MPa or higher and 1.5 MPa or lower, and further preferably 0.1 MPa or higher and 1.0 MPa or lower.

[0130] In order to produce the high-density polyethylene (A), a co-catalyst is preferably used and is added in order to exhibit polymerization activity by reducing the titanium source.

[0131] As a cocatalyst, for example, triethylaluminum, triisobutylaluminum, diethylaluminum chloride, ethylaluminum sesquichloride, ethylaluminum dichloride, etc. can be cited. Particularly preferred are triethylaluminum and triisobutylaluminum. In addition, by adding two cocatalysts with different reducibility to a polymerization reactor at the same time, a polymerization reaction is carried out under a state with a plurality of active sites to generate a trace of low molecular weight components and high molecular weight components, so that the compatibility with the low density polyethylene (B) described later is improved, so it is preferred.

[0132] As a method for adjusting the molecular weight of the high-density polyethylene (A), for example, there can be cited: a method of allowing hydrogen to exist in the polymerization system and a method of changing the polymerization temperature as described in the specification of German Patent Application Publication No. 3127133. By adding hydrogen as a chain transfer agent in the polymerization system, the molecular weight can be controlled within an appropriate range.

[0133] As a method for adjusting the density of the high-density polyethylene (A), for example, there is a method of allowing the above-mentioned comonomer to exist in the polymerization system. By adding the comonomer in the polymerization system, the density can be controlled within an appropriate range.

[0134] Examples of the solvent separation method include decantation, centrifugal separation, and filtration. Among them, centrifugal separation is more preferred because it has a good separation efficiency between the ethylene polymer and the solvent.

[0135] The polymerized powder of high density polyethylene (A) is granulated into granules by using single screw extruder, twin screw extruder, exhaust extruder, tandem extruder etc. The type of extruder and the number of extrusions are not particularly limited, and it is preferred to utilize a twin screw extruder for mixing. In addition, by adding a low density polyethylene (B) described later of about 5 mass % relative to the powder obtained by slurry polymerization when utilizing a twin screw extruder for mixing, the compatibility with the low density polyethylene (B) is improved in the mixing process afterwards, so it is preferred.

[0136] (Method for producing low-density polyethylene)

[0137] As the low-density polyethylene (B), a high-pressure process low-density polyethylene is preferred.

[0138] High pressure low density polyethylene can be obtained by free radical polymerization of ethylene in an autoclave reactor or a tubular reactor, but there is no particular limitation. In the case of an autoclave reactor, the polymerization conditions are set to a temperature of 200°C to 300°C and a polymerization pressure of 100MPa to 250MPa in the presence of a peroxide, while in the case of a tubular reactor, the polymerization conditions are set to a polymerization reaction peak temperature of 180°C to 400°C and a polymerization pressure of 100MPa to 400MPa in the presence of a peroxide and a chain transfer agent.

[0139] The physical properties of the obtained low-density polyethylene (B) can be controlled by adjusting the polymerization temperature, polymerization pressure, the type of peroxide, and the presence or absence of a chain transfer agent.

[0140] The peroxide is not particularly limited, and examples thereof include methyl ethyl ketone peroxide, peroxyketals (specifically, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)octane, 4,4-bis(tert-butylperoxy)butyl valerate, 2,2-bis(tert-butylperoxy)butane, etc.), hydroperoxides (specifically, tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, p-menthane, etc.) peroxide, 1,1,3,3-tetramethylbutyl hydroperoxide, etc.), dialkyl peroxides (specifically, di-tert-butyl peroxide, dicumyl peroxide, bis(tert-butylperoxyisopropyl)benzene, tert-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyldi(tert-butylperoxy)-3-hexyne, etc.), diacyl peroxides (specifically, acetyl peroxide, isobutyryl peroxide, octanoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, etc.), peroxydicarbonates (specifically, diisopropyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl) peroxydicarbonate, di(methoxyisopropyl) peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, diallyl peroxydicarbonate, etc.), peroxyesters (specifically, tert-butyl peroxyacetate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, tert-butyl peroxy tert-Butyl peroxyoctanoate, tert-Butyl peroxyneodecanoate, cumyl peroxyneodecanoate, tert-Butyl peroxy-2-ethylhexanoate, tert-Butyl peroxy-3,5,6-trimethylhexanoate, tert-Butyl peroxylaurate, tert-Butyl peroxybenzoate, tert-Butyl peroxyisopropyl carbonate, cumyl peroxyoctanoate, tert-Hexyl peroxyneodecanoate, tert-Hexyl peroxypivalate, tert-Butyl peroxyneohexanoate, tert-Hexyl peroxyneohexanoate, cumyl peroxyneohexanoate, etc.), acetyl cyclohexyl sulfonyl peroxide, tert-Butyl peroxyallyl carbonate, etc.

[0141] The chain transfer agent is not particularly limited, and various physical properties can be adjusted by, for example, using a hydrocarbon compound such as propane, propylene, or butane to stop radicals of a growing polymer.

[0142] In addition, the temperature of ethylene supplied to the polymerization reactor and the temperature of the polymer immediately after being discharged from the polymerization reactor affect the branched structure of the polymer. Therefore, as described above, it is preferred to control the temperature of ethylene supplied to the polymerization reactor to 150° C. or more by heating the pipeline immediately before the polymerization reactor with steam. This makes the polymerization reactor a homogeneous state, makes it easy for free radicals to contact the polymer, and easily produces a polymer having a large number of branch points.

[0143] Methods for adjusting the molecular weight and density of low-density polyethylene include, for example, changing the polymerization temperature or pressure, and allowing the above-described chain transfer agent to exist in the polymerization system. By adjusting the above conditions, the molecular weight and density can be controlled within an appropriate range.

[0144] (additive)

[0145] The ethylene resin composition of the present embodiment may further contain additives such as an antioxidant, a light resistance stabilizer, a slip agent, a filler, and an antistatic agent.

[0146] Example

[0147] Hereinafter, the present embodiment will be described in detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples and comparative examples.

[0148] The measuring methods and evaluation methods of various physical properties and characteristics are described below.

[0149] [Measurement methods of physical properties]

[0150] ((Physical Property 1) Melt Flow Rate (MFR) at 190°C and 2.16 kg load)

[0151] The melt flow rate (g / 10 minutes) of each ethylene resin composition and raw material obtained in Examples and Comparative Examples was measured in accordance with JIS K7210 No. D: 1999 (temperature = 190°C, load = 2.16 kg).

[0152] ((Physical Property 2) Density)

[0153] The density (kg / m2) of each ethylene composition and raw material obtained in the examples and comparative examples was measured according to JIS K7112:1999 and the density gradient tube method (23°C). 3 ).

[0154] ((Physical Property 3) ARES Temperature Rise Measurement)

[0155] The storage modulus (G') and loss modulus (G") were measured using ARES-G2 manufactured by TA Instruments with a gap distance of 1 to 2 mm and parallel plates of 8 mm diameter in a nitrogen atmosphere, and their ratio G" / G' was defined as tan δ.

[0156] The ethylene resin compositions of the embodiments and comparative examples described later are completely melted by heating them for 10 to 30 minutes in a device set at 200°C. Then, the temperature is lowered from 200°C to 30°C at a rate of 5°C / min. When cooling, the distance between the plates is adjusted so that the normal stress is zero, taking into account the shrinkage of the sample and the fixture due to thermal expansion. Next, the dynamic viscoelasticity is measured while the temperature is raised from 30°C to 150°C at a rate of 5°C / min. The measurement is performed while the strain amount changes between 0.1% and 5.0% according to the softening of the resin as the temperature rises. The strain is measured starting from 0.1% and changes according to the softening of the ethylene resin composition. Specifically, the strain is increased in a manner such that the torque is not less than 1g·cm. The strain at 30°C is 0.1%, and the strain at 150°C is 5.0%.

[0157] Device: ARES-G2 (manufactured by TA Instruments)

[0158] Atmosphere: Nitrogen

[0159] Geometry: 8mmφ parallel plate

[0160] Gap: 1.0mm~2.0mm

[0161] Strain: 0.1% to 5.0% (varies depending on the state)

[0162] Measuring temperature: 30℃~150℃

[0163] Heating / cooling speed: 5℃ / minute

[0164] The tan δ obtained by the ARES temperature increase measurement was calculated, and the temperature (°C) at which the average value (M+m) / 2 of the maximum value M and the minimum value m was reached was calculated. In addition, the value of tan δ at 150°C was determined.

[0165] ((Physical Property 4) Determination of Melt Viscosity)

[0166] The melt viscosity of the ethylene resin compositions of Examples and Comparative Examples described below was measured using Capilograph 1D manufactured by Toyo Seiki Co., Ltd., using a capillary having a capillary length of 50.80 mm and a capillary diameter of 0.77 mm and a piston descending speed of 0.15 mm / min to 40.00 mm / min.

[0167] The measurement was performed under the temperature conditions of 170°C and 230°C.

[0168] The shear rate is calculated from the piston descending speed and the capillary diameter. -1The melt viscosity measured under the conditions of 230°C and a shear rate of 10 s is set to X (Pa·s). -1 The melt viscosity measured under the conditions is set to Y (Pa·s), and the value of (YX) / (170-230) is calculated.

[0169] ((Physical Property 5) DSC Measurement)

[0170] Differential scanning calorimetry (DSC) was performed using a DSC-7 differential scanning calorimeter manufactured by PerkinElmer, and a DSC curve (temperature-heat flow curve) was obtained under the following conditions according to the following procedures.

[0171] (1) About 5 mg of the ethylene resin composition produced in Examples and Comparative Examples was placed in an aluminum pan, the temperature was raised to 200° C. at a rate of 200° C. / min, and the temperature was maintained at 200° C. for 5 minutes.

[0172] (2) Next, the temperature was lowered from 200°C to 50°C at a rate of 10°C / min and maintained for 5 minutes after the temperature reduction was completed.

[0173] (3) Next, the temperature is increased from 50°C to 200°C at a rate of 10°C / min.

[0174] Based on the DSC curve observed in the process of (3) above, the highest temperature at the melting peak position was taken as the melting point (°C).

[0175] In the DCS curve, the number of melting peaks, the melting peak temperature (° C.) on the highest temperature side, and the difference (° C.) between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side were calculated.

[0176] [Evaluation method]

[0177] ((Evaluation 1) FE number)

[0178] The ethylene resin composition was molded using a T-die film-making machine (HM40N manufactured by Hokushin Sangyo Co., Ltd., with a screw diameter of 40 mm and a die width of 300 mm) at a barrel temperature of 200°C, a die temperature of 210°C and an extrusion rate of 5 kg / hour.

[0179] Both ends were trimmed by 50 mm to obtain a film of the ethylene resin composition having a thickness of 35 μm. The film area of ​​400 cm was visually evaluated. 2 The number of FEs in which the length of the major axis is greater than 0.1 mm is N3.

[0180] Using the number N1 (pieces) of FEs of a single high-density polyethylene (A) film as a raw material, the mass proportion a of the high-density polyethylene (A) when the overall ethylene resin composition is set to 1, the number N2 (pieces) of FEs of a single low-density polyethylene (B) film as a raw material, and the mass proportion b of the low-density polyethylene (B) when the overall ethylene resin composition is set to 1, the FE index X is defined by "X = N3 / (N1×a+N2×b)" and evaluated as described below.

[0181] In addition, when two or more low-density polyethylenes (B) are used, the term of the low-density polyethylene as the denominator is increased according to the number.

[0182] ◎: 0.5 or less

[0183] ○: greater than 0.5 and less than or equal to 0.7

[0184] △: greater than 0.7 and less than or equal to 1.0

[0185] ×: greater than 1.0

[0186] ((Evaluation 2) Evaluation of heat shrinkage resistance)

[0187] The film obtained in the above (Evaluation 1) was cut into a piece of 5 cm in width×5 cm in length, and a heat shrinkage resistance test was performed in an environment of 130° C., 2 atmospheres, and 100% RH.

[0188] The temperature was raised from room temperature to 130°C, and then maintained at 130°C for 20 minutes. The sample was then removed after decompression and cooling for 5 minutes. When the length of the side with the largest shrinkage was set as L (cm), the heat shrinkage rate (%) was calculated by (5-L) / 5×100, and evaluated according to the following criteria.

[0189] ◎: Less than 20%

[0190] ○: 20% or more and less than 30%

[0191] △: greater than or equal to 30% and less than 40%

[0192] ×: More than 40%

[0193] ((Evaluation 3) Evaluation of strength retention at high temperature)

[0194] The film obtained in the above (Evaluation 1) was cut into 5 cm width×5 cm length, and the four corners of the film were attached to a slide glass using double-sided tape cut into 0.5 cm width×0.5 cm length to prepare a sample.

[0195] The samples were subjected to a strength retention evaluation test under an environment of 150° C., 2 atmospheres, and 100% RH.

[0196] The temperature was raised from room temperature to 150°C and then maintained at 150°C for 20 minutes.

[0197] After the sample was taken out, a scratch test was performed within 5 minutes according to the method described in JIS K5600-5-4.

[0198] The surface of the slide glass after the test was observed using a pencil having a hardness of F, and the strength retention at high temperature was evaluated according to the following criteria.

[0199] ○: No scratches were observed on the slide glass.

[0200] △: Slight scratches were observed on the slide glass.

[0201] ×: A large number of scratches were observed on the slide glass.

[0202] ((Evaluation 4) 20° gloss)

[0203] The glossiness of 10 film samples randomly cut out from the film obtained in the above (Evaluation 1) was measured at an incident angle of 20° using GLOSS METER GM-26D manufactured by Murakami Color Research Laboratory Co., Ltd. in accordance with ASTM D523 (2457).

[0204] The average value of the obtained glossiness values ​​was used as an index of blocking resistance and evaluated as follows.

[0205] ◎: Less than 15.0%

[0206] ○: 15.0% or more and less than 30.0%

[0207] △: 30.0% or more and less than 45.0%

[0208] ×: 45.0% or more

[0209] [Preparation of components used in Examples and Comparative Examples]

[0210] (High-density polyethylene (A))

[0211] <Preparation of Ziegler-Natta catalyst (a)>

[0212] 1000 mL of a 2 mol / L hexane solution of hydroxytrichlorosilane was placed in an 8 L stainless steel autoclave that had been fully purged with nitrogen, and AlMg5(C4H9) was added dropwise over 4 hours while stirring at 65°C. 11 2550 mL of a hexane solution of an organic magnesium compound represented by (OC4H9)2 (corresponding to 2.68 mol of magnesium) was added, and then the reaction was continued while stirring at 65°C for 1 hour.

[0213] After the reaction was completed, the supernatant was removed and washed four times with 1800 mL of hexane to obtain a solid as a carrier. The solid was analyzed to find that the amount of magnesium contained in 1 g of the solid was 8.31 mmol.

[0214] To 1970 mL of hexane slurry containing 110 g of the above-mentioned carrier, 110 mL of a 1 mol / L hexane solution of titanium tetrachloride and 1 mol / L of AlMg5(C4H9) were added simultaneously under stirring at 10°C for 1 hour. 11 110 mL of a hexane solution of an organomagnesium compound represented by (OSiH)2 was added and the reaction was continued at 10°C for 1 hour. After the reaction was completed, 1100 mL of the supernatant was removed and washed twice with 1100 mL of hexane to prepare a Ziegler-Natta catalyst (a).

[0215] <Preparation of Metallocene Catalyst (b)>

[0216] The average particle size is 15 μm and the surface area is 70 m 2 Spherical silica having an internal pore volume of 1.8 mL / g and calcined at 500° C. for 5 hours in a nitrogen atmosphere was dehydrated to obtain dehydrated silica.

[0217] The amount of surface hydroxyl groups of the dehydrated silica was 1.85 mmol / g per 1 g of SiO2.

[0218] Under nitrogen atmosphere, 40 g of the above dehydrated silica was dispersed in 800 mL of hexane in an autoclave with a capacity of 1.8 L, thereby obtaining a slurry. 80 mL of a hexane solution of triethylaluminum (concentration: 1 mol / L) was added to the obtained slurry while maintaining the temperature at 50° C. under stirring, and then stirred for 2 hours to react the triethylaluminum with the surface hydroxyl groups of the silica, thereby obtaining a component containing the silica treated with triethylaluminum and a supernatant, wherein the surface hydroxyl groups of the silica treated with triethylaluminum were capped with triethylaluminum.

[0219] Then, the supernatant in the obtained reaction mixture was removed by decantation, thereby removing unreacted triethylaluminum in the supernatant.

[0220] Then, an appropriate amount of hexane was added to obtain 880 mL of hexane slurry of silica (component [c]) treated with triethylaluminum.

[0221] On the other hand, 200 mmol of [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]titanium-1,3-pentadiene (hereinafter referred to as "titanium complex") was dissolved in 1000 mL of Isopar E (a trade name of a hydrocarbon mixture manufactured by Exxon Chemical Company (USA)), and AlMg6(C2H5)3(n-C4H9) prepared in advance from triethylaluminum and dibutylmagnesium was added. y 20 mL of a 1 mol / L hexane solution was added, and then hexane was added to adjust the titanium complex concentration to 0.1 mol / L, thereby obtaining component [d].

[0222] Separately, 5.7 g of bis(hydrogenated tallow)methylammonium-tris(pentafluorophenyl)(4-hydroxyphenyl)borate (hereinafter referred to as "borate compound") was added and dissolved in 50 mL of toluene to obtain a 100 mmol / L toluene solution of the borate compound. 5 mL of a 1 mol / L hexane solution of ethoxydiethylaluminum was added to the toluene solution of the borate compound at room temperature, and then hexane was added to adjust the borate concentration in the solution to 70 mmol / L. Then, the mixture was stirred at room temperature for 1 hour to obtain a reaction mixture containing the borate compound.

[0223] 46 mL of the reaction mixture containing the borate compound was added to 800 mL of the slurry of component [c] obtained above while stirring at 15°C to 20°C to load the borate compound on silica. In this way, a slurry of silica loaded with borate compound was obtained. Then 32 mL of component [d] obtained above was added and stirred for 3 hours to react the titanium complex with the borate compound. In this way, a supported metallocene catalyst (b) containing silica and a supernatant and having a catalytically active substance formed on the silica was obtained.

[0224] <Manufacturing of high-density polyethylene (A-1)>

[0225] A 280 L container-type polymerization reactor equipped with a stirring device was used to continuously polymerize at a polymerization temperature of 80° C., a polymerization pressure of 0.80 MPa, and an average residence time of 1.6 hours. Dehydrated n-hexane was supplied as a solvent at 40 L / hour, the above-mentioned Ziegler-Natta catalyst [a] was supplied as a catalyst at 0.4 g / hour, triisobutylaluminum as a liquid co-catalyst component was supplied at 12 mmol / hour in terms of Al atoms, and triethylaluminum was supplied at 12 mmol / hour in terms of Al atoms. Hydrogen gas for molecular weight adjustment was supplied in a gas phase concentration of 40.2 mol% relative to ethylene and 1-butene, and 1-butene was supplied in a gas phase concentration of 0.52 mol% relative to ethylene, thereby polymerizing ethylene and 1-butene.

[0226] Dehydrated n-hexane was supplied from the bottom of the polymerization reactor, hydrogen was supplied from the middle between the liquid surface and the bottom of the polymerization reactor together with the catalyst from the catalyst introduction line in order to contact the catalyst in advance, and ethylene was supplied from the bottom of the polymerization reactor.

[0227] The polymerization slurry in the polymerization reactor was introduced into a flash tank at a pressure of 0.08 MPa and a temperature of 75° C. so that the liquid level in the polymerization reactor was kept constant, and unreacted ethylene, 1-butene and hydrogen were separated.

[0228] Next, the polymerized slurry was continuously sent to a centrifuge so that the liquid level in the polymerization reactor was kept constant, and the polymer was separated from the solvent and the like. The content of the solvent and the like relative to the polymer at this time was 45%.

[0229] The separated high-density polyethylene powder was dried at 85° C. while blowing nitrogen.

[0230] Next, 300 ppm by mass of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] as an antioxidant was added to the obtained powder, and then 5% by mass of pellets of the low-density polyethylene (B-1) described below were added, and melt-kneaded and granulated at a temperature of 200°C using a TEX-44 twin-screw extruder manufactured by The Japan Steel Works, Ltd., to obtain a high-density polyethylene (A-1).

[0231] The density of the obtained high-density polyethylene (A-1) was 960 kg / m 3 , MFR is 10.0g / 10min.

[0232] <Manufacturing of high-density polyethylene (A-2)>

[0233] High-density polyethylene (A-2) was obtained by performing the same operation as the high-density polyethylene (A-1) except that the low-density polyethylene (B-1) was not added to the polymer powder. The density of the obtained high-density polyethylene (A-2) was 965 kg / m 3 , MFR is 12.0g / 10min.

[0234] <Manufacturing of high-density polyethylene (A-3)>

[0235] A high-density polyethylene (A-3) was obtained by the same operation as in the high-density polyethylene (A-1) except that triisobutylaluminum was supplied as a liquid co-catalyst component at 24 mmol / hr in terms of Al atoms.

[0236] The density of the obtained high-density polyethylene (A-3) is 960 kg / m 3, MFR is 11.0g / 10min.

[0237] <Manufacturing of high-density polyethylene (A-4)>

[0238] High-density polyethylene (A-4) was obtained by carrying out the same operation as that of the above-mentioned high-density polyethylene (A-1), except that triisobutylaluminum was supplied as a liquid co-catalyst component at 24 mmol / h in terms of Al atoms and low-density polyethylene (B-1) was not added to the polymerization powder.

[0239] The density of the obtained high-density polyethylene (A-4) is 960 kg / m 3 , MFR is 11.0g / 10min.

[0240] <Manufacturing of high-density polyethylene (A-5)>

[0241] High-density polyethylene (A-5) was obtained by performing the same operations as those for the above-mentioned high-density polyethylene (A-1), except that hydrogen for adjusting the molecular weight was supplied in a manner such that the gas phase concentration was 20.2 mol % relative to ethylene and 1-butene, and 1-butene was supplied in a manner such that the gas phase concentration was 0.96 mol % relative to ethylene.

[0242] The density of the obtained high-density polyethylene (A-5) is 945 kg / m 3 , MFR is 5.0g / 10min.

[0243] <Manufacturing of high-density polyethylene (A-6)>

[0244] A high-density polyethylene (A-6) was produced by carrying out continuous secondary polymerization using the prepared supported metallocene catalyst (b), a liquid co-catalyst component, hexane as a solvent, and ethylene as a monomer.

[0245] In the first stage reaction polymerizer, the temperature was 60°C, the total pressure was 0.25 MPa, the gas phase concentration of 1-butene relative to ethylene was 0.05 mol%, and the gas phase concentration of hydrogen relative to ethylene and 1-butene was 0.13 mol%.

[0246] In the second stage reaction polymerizer, the temperature was 75°C, the total pressure was 0.85 MPa, the gas phase concentration of 1-butene relative to ethylene was 1.2 mol%, and the gas phase concentration of hydrogen relative to ethylene and 1-butene was 0.11 mol%.

[0247] The obtained high-density polyethylene powder was melt-kneaded and pelletized at 200° C. using a TEX-44 twin-screw extruder manufactured by The Japan Steel Works, Ltd. without using any additives such as a neutralizer and an antioxidant, thereby obtaining a high-density polyethylene (A-6).

[0248] The density of the obtained high-density polyethylene (A-6) is 941 kg / m 3 , MFR is 1.0g / 10min.

[0249] <Manufacturing of high-density polyethylene (A-7)>

[0250] Hydrogen gas for molecular weight adjustment was supplied in a gas phase concentration of 60.2 mol% relative to ethylene and 1-butene, and 1-butene was not used. High-density polyethylene (A-7) was obtained by the same operation as that of high-density polyethylene (A-1) under other conditions.

[0251] The density of the obtained high-density polyethylene (A-7) is 965 kg / m 3 , MFR is 28.0g / 10min.

[0252] (Low-density polyethylene (B))

[0253] <Manufacturing of low-density polyethylene (B-1)>

[0254] In an autoclave reactor, the polymerization temperature was 259° C., the polymerization pressure was 128.1 MPa, and tert-butyl peroxyacetate was used as a polymerization initiator to obtain low-density polyethylene (B-1).

[0255] The temperature of ethylene supplied to the polymerization reactor was adjusted to 165° C. by heating the pipe immediately before the polymerization reactor with steam.

[0256] The obtained low-density polyethylene (B-1) was processed into pellets using a single-screw extruder. The density was 920 kg / m 3 , MFR is 2.0g / 10min.

[0257] <Manufacturing of low-density polyethylene (B-2)>

[0258] In a tubular reactor, polymerization was carried out at a polymerization temperature of 280° C. and a polymerization pressure of 200 MPa, using tert-butyl peroxy-2-ethylhexanoate as a polymerization initiator, and 1.2 mol % of the ethylene raw material was replaced with propylene to obtain a low-density polyethylene (B-2).

[0259] The temperature of ethylene supplied to the polymerization reactor was adjusted to 155° C. by heating the pipe immediately before the polymerization reactor with steam.

[0260] The density of the obtained low-density polyethylene (B-2) is 924 kg / m 3 , MFR is 4.0g / 10min.

[0261] <Manufacturing of low-density polyethylene (B-3)>

[0262] A low-density polyethylene (B-3) was obtained by carrying out the same operation as that of the low-density polyethylene (B-1) except that the pipe immediately before the polymerization reactor was not heated with steam.

[0263] The temperature of ethylene supplied to the polymerization reactor was 115°C.

[0264] The density of the obtained low-density polyethylene (B-3) is 920 kg / m 3 , MFR is 2.0g / 10min.

[0265] <Manufacturing of low-density polyethylene (B-4)>

[0266] The polymerization temperature was 245°C, the polymerization pressure was 170.0 MPa, 18.5 mol% of the ethylene raw material was changed to butane, and the pipeline immediately before the polymerization reactor was not heated. Except for this, the same operations as those for low-density polyethylene (B-1) were performed to obtain low-density polyethylene (B-4).

[0267] The temperature of ethylene supplied to the polymerization reactor was 110°C.

[0268] The density of the obtained low-density polyethylene (B-4) is 923 kg / m 3 , MFR is 3.8g / 10min.

[0269] <Manufacturing of low-density polyethylene (B-5)>

[0270] The polymerization temperature was 200°C, the polymerization pressure was 150.0 MPa, 7.5 mol% of the ethylene raw material was changed to butane, and the pipeline immediately before the polymerization reactor was not heated. Except for this, the same operations as those for low-density polyethylene (B-1) were performed to obtain low-density polyethylene (B-5).

[0271] The temperature of ethylene supplied to the polymerization reactor was 104°C.

[0272] The density of the obtained low-density polyethylene (B-5) is 931 kg / m 3 , MFR is 5.0g / 10min.

[0273] <Manufacturing of low-density polyethylene (B-6)>

[0274] A low-density polyethylene (B-6) was obtained by carrying out the same operation as that of the low-density polyethylene (B-1) except that the polymerization temperature was changed to 250°C and the polymerization pressure was changed to 110.0 MPa.

[0275] The temperature of ethylene supplied to the polymerization reactor was 161°C.

[0276] The density of the obtained low-density polyethylene (B-6) is 920 kg / m 3 , MFR is 15.0g / 10min.

[0277] (Ethylene resin composition)

[0278] <Example 1 Production of Ethylene Resin Composition (C-1)>

[0279] A single screw extruder (screw diameter: 50 mm, L / D=24) manufactured by Nippon Steel Works, Ltd. was used to melt-knead high-density polyethylene (A-1) and low-density polyethylene (B-1) at 200°C in an amount of 30% by mass of high-density polyethylene (A-1) and 70% by mass of low-density polyethylene (B-1), and granulated into pellets.

[0280] In addition, the variation of the resin pressure was controlled within 5 MPa by adjusting the screw rotation speed of the extruder within the range of 50 rpm to 150 rpm.

[0281] <Example 2 Production of Ethylene Resin Composition (C-2)>

[0282] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-2) and the low-density polyethylene (B-2) were adjusted to 20% by mass and 80% by mass, respectively.

[0283] <Example 3 Production of Ethylene Resin Composition (C-3)>

[0284] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-3) and the low-density polyethylene (B-1) were adjusted to 30% by mass and 70% by mass, respectively.

[0285] <Example 4 Production of Ethylene Resin Composition (C-4)>

[0286] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-4) and the low-density polyethylene (B-2) were adjusted to 40% by mass and 60% by mass, respectively.

[0287] <Example 5 Production of Ethylene Resin Composition (C-5)>

[0288] The high-density polyethylene (A-1) and the low-density polyethylene (B-3) are adjusted to 30% by mass and 70% by mass, respectively, and the screw speed of the extruder is kept constant at 100 rpm. In addition, melt mixing is carried out by the same operation as the above-mentioned ethylene resin composition (C-1), and granulation is carried out into pellets.

[0289] <Example 6 Production of Ethylene Resin Composition (C-6)>

[0290] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-1) and the low-density polyethylene (B-4) were adjusted to 30% by mass and 70% by mass, respectively.

[0291] <Example 7 Production of Ethylene Resin Composition (C-7)>

[0292] The high-density polyethylene (A-2) and the low-density polyethylene (B-2) are adjusted to 10% by mass and 90% by mass, respectively, and the screw speed of the extruder is kept constant at 100 rpm. In addition, melt mixing is carried out by the same operation as the above-mentioned ethylene resin composition (C-1), and granulation is carried out into pellets.

[0293] <Example 8 Production of Ethylene Resin Composition (C-8)>

[0294] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-1) and the low-density polyethylene (B-1) were adjusted to 55% by mass and 45% by mass, respectively.

[0295] <Example 9 Production of Ethylene Resin Composition (C-9)>

[0296] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-5) and the low-density polyethylene (B-3) were adjusted to 35% by mass and 65% by mass, respectively.

[0297] <Comparative Example 1 Preparation of Ethylene Resin Composition (C-10)>

[0298] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-1) and the low-density polyethylene (B-1) were adjusted to 70% by mass and 30% by mass, respectively.

[0299] <Comparative Example 2: Production of Ethylene Resin Composition (C-11)>

[0300] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-6) and the low-density polyethylene (B-1) were adjusted to 40% by mass and 60% by mass, respectively.

[0301] <Comparative Example 3: Production of Ethylene Resin Composition (C-12)>

[0302] The mixture was melt-kneaded and granulated into pellets in the same manner as the ethylene resin composition (C-1) except that the high-density polyethylene (A-4) and the low-density polyethylene (B-4) were adjusted to 30% by mass and 70% by mass, respectively.

[0303] <Comparative Example 4: Production of Ethylene Resin Composition (C-13)>

[0304] The high-density polyethylene (A-2) and the low-density polyethylene (B-4) are adjusted to 40% by mass and 60% by mass, respectively, and the screw speed of the extruder is kept constant at 100 rpm. In addition, melt mixing is carried out by the same operation as the above-mentioned ethylene resin composition (C-1), and granulation is carried out into pellets.

[0305] <Comparative Example 5: Production of Ethylene Resin Composition (C-14)>

[0306] The high-density polyethylene (A-7) and the low-density polyethylene (B-6) are adjusted to 45% by mass and 55% by mass, respectively, and the screw speed of the extruder is kept constant at 100 rpm. In addition, melt mixing is carried out by the same operation as the above-mentioned ethylene resin composition (C-1), and granulation is carried out into pellets.

[0307] <Comparative Example 6 Preparation of Ethylene Resin Composition (C-15)>

[0308] The low-density polyethylene (B-5) was melt-kneaded using a single-screw extruder (screw diameter: 50 mm, L / D=24) manufactured by Nippon Steel Works, Ltd. at a screw speed of 100 rpm and 200° C. and granulated into pellets.

[0309] <Comparative Example 7: Production of Ethylene Resin Composition (C-16)>

[0310] The high-density polyethylene (A-6) and the low-density polyethylene (B-5) are adjusted to 70% by mass and 30% by mass, respectively, and the screw speed of the extruder is kept constant at 100 rpm. In addition, melt mixing is carried out by the same operation as the above-mentioned ethylene resin composition (C-1), and granulation is carried out into pellets.

[0311] <Comparative Example 8 Preparation of Ethylene Resin Composition (C-17)>

[0312] An ethylene resin composition (C-17) was obtained by the same method as in Example 2 described in Japanese Patent No. 6912290.

[0313] <Comparative Example 9: Production of Ethylene Resin Composition (C-18)>

[0314] An ethylene resin composition (C-18) was obtained by the same method as in Example 9 described in Japanese Patent No. 6912290.

[0315] <Comparative Example 10: Production of Ethylene Resin Composition (C-19)>

[0316] An ethylene resin composition (C-19) was obtained by the same method as in Example 3 described in Japanese Patent No. 6243195.

[0317]

[0318]

[0319] Industrial Applicability

[0320] The ethylene resin composition of the present invention has industrial applicability as a raw material for protective films and the like in film applications where fisheye quality is particularly important.

Claims

1. An ethylene resin composition, wherein The ethylene resin composition satisfies the following <Condition (A)> to <Condition (D)>: <Condition (A)> The melt flow rate of the ethylene resin composition under the conditions of 190° C. and a load of 2.16 kg is 1.0 g / 10 min or more and 20.0 g / 10 min or less; <Condition (B)> The density of the ethylene resin composition is 920 kg / m 3 Above and 945kg / m 3 the following; <Condition (C)> In the ARES temperature rise measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 115°C to 145°C. <Condition (D)> In the ARES temperature rise measurement, the value of tan δ at 150°C is 1.00 or more and 1.50 or less, The ethylene resin composition contains 10 mass % or more and 30 mass % or less of a 3 High density polyethylene above.

2. The ethylene resin composition according to claim 1, wherein The ethylene resin composition has a melt flow rate of 2.0 g / 10 min or more and 15.0 g / 10 min or less under the conditions of 190° C. and a load of 2.16 kg.

3. The ethylene resin composition according to claim 1 or 2, wherein The ethylene resin composition has a melt flow rate of 3.0 g / 10 min or more and 10.0 g / 10 min or less under the conditions of 190° C. and a load of 2.16 kg.

4. The ethylene resin composition according to claim 1 or 2, wherein The density of the ethylene resin composition is 928 kg / m 3 Above 943kg / m 3 the following.

5. The ethylene resin composition according to claim 1 or 2, wherein The density of the ethylene resin composition is 930 kg / m 3 Above and 940kg / m 3 the following.

6. The ethylene resin composition according to claim 1 or 2, wherein In the ARES temperature rise measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 118°C to 140°C.

7. The ethylene resin composition according to claim 1 or 2, wherein In the ARES temperature rise measurement, the temperature at which the average value (M+m) / 2 of the maximum value M and the minimum value m of tan δ in the temperature range of 30°C to 150°C is reached is 120°C to 135°C.

8. The ethylene resin composition according to claim 1 or 2, wherein In the ARES temperature rise measurement, the value of tan δ at 150° C. is 1.05 or more and 1.40 or less.

9. The ethylene resin composition according to claim 1 or 2, wherein In the ARES temperature rise measurement, the value of tan δ at 150° C. is 1.10 or more and 1.30 or less.

10. The ethylene resin composition according to claim 1 or 2, wherein When the temperature is 170℃ and the shear rate is 10s -1 The melt viscosity of the ethylene resin composition measured under the conditions of At 230°C and a shear rate of 10 s -1 When the melt viscosity of the ethylene resin composition measured under the conditions of is denoted as Y (Pa·s), Satisfies the following formula (1): 5≤(YX) / (170-230)≤25……(1).

11. The ethylene resin composition according to claim 10, wherein The (YX) / (170-230) is greater than 7 and less than 22.

12. The ethylene resin composition according to claim 10, wherein The (YX) / (170-230) is 10 or more and 20 or less.

13. The ethylene resin composition according to claim 1 or 2, wherein In the temperature-heat flow curve of the ethylene resin composition obtained by differential scanning calorimetry (DSC), there are two or more melting peaks, the melting peak temperature on the highest temperature side is 118° C. or more, and The difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is 10° C. or more and 30° C. or less.

14. The ethylene resin composition according to claim 13, wherein The difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is 12° C. or more and 28° C. or less.

15. The ethylene resin composition according to claim 13, wherein The difference between the melting peak temperature on the highest temperature side and the melting peak temperature on the lowest temperature side is 15° C. or more and 25° C. or less.

16. The ethylene resin composition according to claim 1 or 2, wherein The ethylene resin composition has a density of 942 kg / m 3 The above high-density polyethylene has a density of 930kg / m 3 A mixture of the following low density polyethylene.

17. The ethylene resin composition according to claim 1 or 2, wherein The content of the high-density polyethylene is 15% to 30% by mass.

18. The ethylene resin composition according to claim 1 or 2, wherein The content of the high-density polyethylene is 20% to 30% by mass.

19. The ethylene resin composition according to claim 16, wherein The low-density polyethylene is a low-density polyethylene selected from the group consisting of high-pressure low-density polyethylene, linear low-density polyethylene and ultra-low-density polyethylene.

20. The ethylene resin composition according to claim 16, wherein The polyethylene contained in the ethylene resin composition is an ethylene homopolymer or a copolymer of ethylene and α-olefin.

21. The ethylene resin composition according to claim 20, wherein The α-olefin is a compound selected from the group consisting of propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.

22. A molded body, wherein The molded article is a molded article of the ethylene resin composition according to any one of claims 1 to 21.

23. The molded article according to claim 22, wherein The shaped body is a film.

24. The molded article according to claim 23, wherein The film is a multi-layer film, and the ethylene-based resin composition is used for the outermost layer.

25. The molded article according to claim 23, wherein The film is a multi-layer film, and the ethylene-based resin composition is used for an intermediate layer.