Polyvinyl alcohol / modified glass fiber composite material and preparation method thereof

By modifying the glass fiber surface, forming hydrogen bond interaction with polyvinyl alcohol, the problem of insufficient bonding force between the fiber and the matrix is ​​solved, significantly improving the mechanical properties and toughness of the composite material, and achieving high strength and high transparency The effect of overreach.

CN116162318BActive Publication Date: 2024-11-05JIANGXI GANNING JINKO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310321299.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-11-05
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The interface bonding force between the fiber and the matrix is ​​weak, which limits the performance of the fiber's high performance and leads to low mechanical strength of the composite material.

Method used

通过对玻璃纤维进行改性处理,引入氨基、羧基或羟基等活性基团,增强其表面粗糙度和表面能,形成与聚乙烯醇中的羟基氢键相互作用,从而提高纤维与基体的界面相容性和力学性能。

Benefits of technology

It significantly improves the mechanical properties of the composite material, increases the tensile strength by 300%, and forms an internal crosslinked structure, which enhances the toughness and transmittance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004151797530000021
    Figure BDA0004151797530000021
  • Figure BDA0004151797530000022
    Figure BDA0004151797530000022
  • Figure BDA0004151797530000023
    Figure BDA0004151797530000023
Patent Text Reader

Abstract

The present invention discloses a polyvinyl alcohol / modified glass fiber composite material, wherein the composite material is composed of a polyvinyl alcohol matrix and a modified glass fiber bonded to the polyvinyl alcohol matrix through hydrogen bonding; the modified glass fiber is an amino glass fiber, a carboxylated glass fiber or a hydroxylated glass fiber. The present invention also discloses a method for preparing the polyvinyl alcohol / modified glass fiber composite material. The composite material of the present invention uses polyvinyl alcohol as a matrix material, and obtains an amino, carboxylated, or hydroxylated glass fiber by surface pretreatment and surface functional group modification of the glass fiber. The functional group can enhance the surface roughness and surface energy of the glass fiber, thereby improving the composite effect and compatibility of the glass fiber and the matrix material, and further enhancing the mechanical properties of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyvinyl alcohol / modified glass fiber composite material and also relates to a preparation method of the composite material. Background Art

[0002] The performance of fiber-reinforced composites depends on the mechanical properties of the polymer matrix, the load-bearing capacity of the fiber, and the interface compatibility between the polymer matrix and the fiber. However, the interfacial bonding between the fiber and the matrix is ​​weak, which limits the high performance of the fiber and makes the composite material show extremely low mechanical strength.

[0003] Polyvinyl alcohol (PVA) has good water solubility and biocompatibility and is one of the most widely used synthetic polymer materials. Its molecular structure contains many hydroxyl groups, which provide abundant interaction sites for the formation of hydrogen bonds, making it possible to further strengthen and toughen and functionalize. At the same time, PVA has excellent mechanical properties, chemical stability and film-forming properties, making it an ideal matrix material for studying the mechanism of glass fiber reinforcement. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a polyvinyl alcohol / modified glass fiber composite material, in which the glass fiber is first modified and then the modified glass fiber is compounded with polyvinyl alcohol. The surface modification of the glass fiber can effectively improve the interfacial bonding strength and compatibility between the fiber and the matrix, thereby greatly improving the mechanical properties of the composite material. Another purpose of the present invention is to provide a method for preparing the above-mentioned polyvinyl alcohol / modified glass fiber composite material.

[0005] Technical solution: The polyvinyl alcohol / modified glass fiber composite material of the present invention comprises a polyvinyl alcohol matrix and modified glass fibers bonded to the polyvinyl alcohol matrix through hydrogen bonding; the modified glass fibers are amino glass fibers, carboxylated glass fibers or hydroxylated glass fibers.

[0006] Wherein, the mass ratio of the polyvinyl alcohol matrix to the modified glass fiber is 5-7:1.

[0007] Wherein, the length of the modified glass fiber is 10-20 mm and the diameter is 40-50 μm.

[0008] In the composite material of the present invention, the matrix material polyvinyl alcohol contains a large amount of hydroxyl groups, and the glass fiber used for filling and reinforcement is surface-modified to introduce active groups amino, carboxyl and hydroxyl groups on its surface. The active groups can form hydrogen bonds with the hydroxyl groups in the polyvinyl alcohol while enhancing the surface roughness and surface energy of the glass fiber, thereby improving the composite effect and compatibility between the glass fiber and the matrix, and further enhancing the mechanical properties of the composite material.

[0009] The preparation method of the polyvinyl alcohol / modified glass fiber composite material comprises the following steps:

[0010] (1) preparing a polyvinyl alcohol (PVA) solution for later use;

[0011] (2) preparing amino glass fiber, carboxylated glass fiber or hydroxylated glass fiber;

[0012] (3) The modified glass fiber is mixed with the polyvinyl alcohol solution, and ultrasonic treatment is performed. The obtained solution after ultrasonic treatment is poured into a mold, and initially frozen at -20-40°C for 2-4 hours. After being taken out and completely thawed, the stretched material is placed at -20-40°C for 2-4 cycles of freeze-thaw; each time freezing is for 8-12 hours, and thawing is performed at room temperature for 1-3 hours. After cyclic freeze-thaw, a polyvinyl alcohol / modified glass fiber composite material is obtained. Cyclic freeze-thaw can form PVA gel. The gelation process of the freeze-thaw cycle method is to shrink the space between polymer chains by freezing the solvent, increase the concentration of the polymer, and form a physical gel, so that a cross-linked network structure can be formed inside the hydrogel without adding any cross-linking agent.

[0013] Wherein, in step (1), the mass concentration of the polyvinyl alcohol solution is 10-20%.

[0014] Wherein, in step (2), the amino-modified glass fiber is prepared by the following method: immersing the pretreated glass fiber in a toluene solution of an aminosilane coupling agent having a mass concentration of 10% to 20%, refluxing at 100 to 120° C. for 12 to 36 hours, filtering, and vacuum drying to obtain the amino-modified glass fiber. The amount of the aminosilane coupling agent is 3% to 5% of the mass of the glass fiber, and the reaction process is as follows:

[0015]

[0016] Wherein, in step (2), the carboxylated glass fiber is prepared by the following method: the pretreated glass fiber is placed in N,N-dimethylacrylamide, after ultrasonic dispersion, it is transferred to an oil bath for stirring, succinic anhydride is added dropwise thereto while stirring, stirring is continued at 50-70°C for 12-36 hours, and the carboxylated glass fiber is obtained after filtering and vacuum drying.

[0017] The mass ratio of glass fiber to succinic anhydride is 1:1-1.5, and the reaction process is as follows:

[0018]

[0019] Wherein, in step (2), the hydroxylated glass fiber is prepared by the following method: immersing the pretreated glass fiber in toluene, ultrasonically dispersing, adding KH560 hydrolyzate thereto, mixing, refluxing at 100-120° C. for 3-5 hours, and then adding a boiled methanol and tetrafluoroboric acid mixture (in the mixture, the volume ratio of methanol to tetrafluoroboric acid is 1-2:

[0020] 1), reflux reaction for 0.5 to 2 hours, then cool to room temperature and add concentrated ammonia water to adjust the solution to neutrality, filter and vacuum dry to obtain hydroxylated glass fiber. The reaction process is as follows:

[0021]

[0022] The pretreatment of the glass fiber is as follows: the glass fiber is placed in acetone, ultrasonically dispersed, and then soaked overnight to remove the surface wetting material. After drying, the glass fiber is then soaked in a concentrated sulfuric acid / hydrogen peroxide mixture and stirred overnight to fully expose the silanol groups on the surface of the glass fiber, and then washed and dried for later use.

[0023] The KH560 hydrolyzate is prepared by mixing KH560, isopropanol and water in a volume ratio of 20:72:8. KH560 is γ-glycidyloxypropyltrimethoxysilane, a coupling agent, and the prepared KH560 hydrolyzate can be used to directly modify glass fibers.

[0024] Wherein, in the concentrated sulfuric acid / hydrogen peroxide mixture, the volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:3.

[0025] The molar ratio of glass fiber to methanol is 0.5:1 to 2:1.

[0026] Wherein, in step (3), the stretching ratio during stretching is 100% to 300%.

[0027] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the composite material of the present invention adopts polyvinyl alcohol (PVA) as the matrix material, and the surface pretreatment of the glass fiber and the modification of the surface functional groups are performed to obtain amino, carboxyl and hydroxylated glass fibers. The functional groups can enhance the surface roughness and surface energy of the glass fiber, thereby improving the composite effect and compatibility of the glass fiber and the matrix material (the active groups on the surface of the modified glass fiber form hydrogen bonds with the hydroxyl groups of PVA), and combined with the stretching-freeze-thaw process, the prepared polyvinyl alcohol / modified glass fiber composite material has the advantages of high strength and good toughness; compared with the polyvinyl alcohol matrix material without the addition of modified glass fiber, the tensile strength of the polyvinyl alcohol / modified glass fiber composite material of the present invention can be increased by up to 300%. DETAILED DESCRIPTION

[0028] Example 1

[0029] The method for preparing the polyvinyl alcohol / modified glass fiber composite material of the present invention comprises the following steps:

[0030] (1) preparing a 10 wt % polyvinyl alcohol (PVA) solution for use; specifically, adding deionized water to a three-necked round-bottom flask, slowly adding a required amount of polyvinyl alcohol solid particles under stirring at room temperature, slowly stirring until there are no lumps, placing the beaker in an oil bath, heating to 60° C., soaking and slowly stirring for 30 min, so that the particles are fully expanded and elastic; then heating to 98° C., boiling, and slowly stirring for 30 min to prepare a 10 wt % PVA solution;

[0031] (2) 10 g of glass fiber was placed in acetone, ultrasonically dispersed for 10 min, and then soaked overnight to remove the surface wetting substances. After drying, the glass fiber was immersed in a mixture of concentrated sulfuric acid / hydrogen peroxide and stirred overnight to fully expose the silanol groups on the surface of the glass fiber. The glass fiber was washed, filtered, and dried for later use. In the mixture of concentrated sulfuric acid / hydrogen peroxide, the volume ratio of concentrated sulfuric acid to hydrogen peroxide was 7:3.

[0032] (3) Preparation of amino glass fiber:

[0033] Immerse 2 g of the glass fiber pretreated in step (2) in a toluene solution of an aminosilane coupling agent having a mass fraction of 10%, and reflux at 100° C. for 36 h. The obtained product is repeatedly washed with toluene, filtered, and vacuum dried to obtain an amino-treated glass fiber;

[0034] Preparation of carboxylated glass fibers:

[0035] 2 g of the glass fiber pretreated in step (2) was placed in N,N-dimethylacrylamide, and after ultrasonic dispersion for 10 min, the mixture was transferred to an oil bath and stirred, and succinic anhydride was added dropwise thereto while stirring. The concentration of succinic anhydride in the reaction solution was 0.4 mol / L. The mixture was stirred at 50° C. for 36 h, and then filtered and vacuum dried to obtain carboxylated glass fiber;

[0036] Preparation of hydroxylated glass fibers:

[0037] 2 g of the glass fiber pretreated in step (2) is immersed in toluene, and after ultrasonic dispersion for 10 min, KH560 hydrolyzate is added thereto (the KH560 hydrolyzate is prepared by mixing KH560, isopropanol and water in a volume ratio of 20:72:8), the amount of KH560 being 3% of the mass of the glass fiber, and the mixture is mixed evenly. After refluxing at 120° C. for 3 h, a boiling methanol and tetrafluoroboric acid mixture is added thereto and refluxed for 0.5 h (the molar ratio of the glass fiber to methanol is 0.5:1), and then the mixture is cooled to room temperature and concentrated ammonia is added dropwise to adjust the solution to neutrality, and the hydroxylated glass fiber is obtained after filtering and vacuum drying;

[0038] (4) The three modified glass fibers prepared in step (3) are mixed with PVA solution respectively, with the mass ratio of polyvinyl alcohol to modified glass fiber being 5:1. After ultrasonic mixing for 1 hour, the obtained solution is poured into a long strip mold, placed at -20°C for preliminary freezing for 4 hours, taken out and completely thawed, stretched and fixed, with a stretching ratio of 100%, and the stretched material is placed at -20°C again for 4 cycles of freeze-thaw, each time freezing for 12 hours and thawing at room temperature for 1 hour. After cyclic freeze-thaw, three polyvinyl alcohol / modified glass fiber composite materials containing different hydrogen bonding effects are obtained.

[0039] Example 2

[0040] The method for preparing the polyvinyl alcohol / modified glass fiber composite material of the present invention comprises the following steps:

[0041] (1) preparing a 15 wt % polyvinyl alcohol (PVA) solution for use; specifically, adding deionized water to a three-necked round-bottom flask, slowly adding polyvinyl alcohol solid particles under stirring at room temperature, slowly stirring until there are no lumps, placing the beaker in an oil bath, heating to 60° C., soaking and slowly stirring for 30 min, so that the particles are fully expanded and elastic; then heating to 98° C., boiling, and slowly stirring for 30 min to prepare a 15 wt % PVA solution;

[0042] (2) 15 g of glass fiber was placed in acetone, ultrasonically dispersed for 20 min, and then soaked overnight to remove the surface wetting material. After drying, the glass fiber was immersed in a mixture of concentrated sulfuric acid / hydrogen peroxide and stirred overnight to fully expose the silanol groups on the surface of the glass fiber. The glass fiber was washed, filtered, and dried for later use. In the mixture of concentrated sulfuric acid / hydrogen peroxide, the volume ratio of concentrated sulfuric acid to hydrogen peroxide was 7:3.

[0043] (3) Preparation of amino glass fiber:

[0044] Immerse 2 g of the glass fiber pretreated in step (2) in a toluene solution of an aminosilane coupling agent having a mass fraction of 15%, reflux at 110° C. for 24 h, filter, and vacuum dry to obtain an amino-treated glass fiber;

[0045] Preparation of carboxylated glass fibers:

[0046] 2 g of the glass fiber pretreated in step (2) was placed in N,N-dimethylacrylamide, and after ultrasonic dispersion for 20 min, it was transferred to an oil bath and stirred, and succinic anhydride was added dropwise thereto while stirring, wherein the concentration of succinic anhydride in the reaction solution was 0.5 mol / L, and stirred at 60° C. for 24 h, and filtered and vacuum dried to obtain carboxylated glass fiber;

[0047] Preparation of hydroxylated glass fibers:

[0048] 2 g of the glass fiber pretreated in step (2) is immersed in toluene, and after ultrasonic dispersion for 20 min, KH560 hydrolyzate is added thereto (the KH560 hydrolyzate is prepared by mixing KH560, isopropanol and water in a volume ratio of 20:72:8), and the amount of KH560 is 3% of the mass of the glass fiber. The mixture is mixed evenly, refluxed at 110° C. for 4 h, and then a boiling methanol and tetrafluoroboric acid mixture is added thereto for reflux reaction for 1 h (the molar ratio of the glass fiber to methanol is 1:1), and then cooled to room temperature and concentrated ammonia is added dropwise to adjust the solution to neutrality, and filtered and vacuum dried to obtain hydroxylated glass fiber;

[0049] (4) The three modified glass fibers prepared in step (3) are mixed with PVA solution respectively, with the mass ratio of polyvinyl alcohol to modified glass fiber being 6:1. After ultrasonic mixing for 2 hours, the obtained solution is poured into a long strip mold, placed at minus 30°C for preliminary freezing for 3 hours, taken out and completely thawed, stretched and fixed, with a stretching ratio of 200%, and the stretched material is placed at minus 30°C again for 3 cycles of freeze-thaw, each time freezing for 10 hours and thawing at room temperature for 2 hours. After cyclic freeze-thaw, three polyvinyl alcohol / modified glass fiber composite materials with different hydrogen bonding effects are obtained.

[0050] Example 3

[0051] The method for preparing the polyvinyl alcohol / modified glass fiber composite material of the present invention comprises the following steps:

[0052] (1) preparing a 20 wt % polyvinyl alcohol (PVA) solution for use; specifically, adding deionized water to a three-necked round-bottom flask, slowly adding polyvinyl alcohol solid particles under stirring at room temperature, slowly stirring until there are no lumps, placing the beaker in an oil bath, heating to 60° C., soaking and slowly stirring for 30 min, so that the particles are fully expanded and elastic; then heating to 98° C., boiling, and slowly stirring for 30 min to prepare a 20 wt % PVA solution;

[0053] (2) 20 g of glass fiber was placed in acetone, ultrasonically dispersed for 30 minutes, and then soaked overnight to remove the surface impregnation material. After drying, the glass fiber was immersed in a mixture of concentrated sulfuric acid / hydrogen peroxide and stirred overnight to fully expose the silanol groups on the surface of the glass fiber. The glass fiber was washed, filtered, and dried for later use. In the mixture of concentrated sulfuric acid / hydrogen peroxide, the volume ratio of concentrated sulfuric acid to hydrogen peroxide was 7:3.

[0054] (3) Preparation of amino glass fiber:

[0055] Immerse 2 g of the glass fiber pretreated in step (2) in a toluene solution of an aminosilane coupling agent having a mass fraction of 20%, reflux at 120° C. for 12 h, filter, and vacuum dry to obtain an amino-treated glass fiber;

[0056] Preparation of carboxylated glass fibers:

[0057] 2 g of the glass fiber pretreated in step (2) was placed in N,N-dimethylacrylamide, and after ultrasonic dispersion for 30 min, the mixture was transferred to an oil bath and stirred, and succinic anhydride was added dropwise thereto while stirring. The concentration of succinic anhydride in the reaction solution was 0.6 mol / L. The mixture was stirred at 70° C. for 12 h, and then filtered and vacuum dried to obtain carboxylated glass fiber;

[0058] Preparation of hydroxylated glass fibers:

[0059] 2 g of the glass fiber pretreated in step (2) is immersed in toluene, and after ultrasonic dispersion for 30 min, KH560 hydrolyzate is added thereto (the KH560 hydrolyzate is prepared by mixing KH560, isopropanol and water in a volume ratio of 20:72:8), and the amount of KH560 is 3% of the mass of the glass fiber. The mixture is mixed evenly, refluxed at 100° C. for 5 h, and then a boiling methanol and tetrafluoroboric acid mixture is added thereto for reflux reaction for 2 h (the molar ratio of the glass fiber to methanol is 2:1), and then cooled to room temperature and concentrated ammonia is added dropwise to adjust the solution to neutrality, and filtered and vacuum dried to obtain hydroxylated glass fiber;

[0060] (4) The three modified glass fibers prepared in step (3) are mixed with PVA solution respectively, with the mass ratio of polyvinyl alcohol to modified glass fiber being 7:1. After ultrasonic mixing for 3 hours, the obtained solution is poured into a long strip mold, placed at -40°C for preliminary freezing for 2 hours, taken out and completely thawed, stretched and fixed, with a stretching ratio of 300%, and the stretched material is placed at -40°C again for two cycles of freeze-thaw, each time freezing for 8 hours, and thawing at room temperature for 3 hours. After the freeze-thaw cycles, three polyvinyl alcohol / modified glass fiber composite materials with different hydrogen bonding effects are obtained.

[0061] Comparative Example 1

[0062] Polyvinyl alcohol is compounded with unmodified glass fiber by:

[0063] (1) preparing a 20 wt % polyvinyl alcohol (PVA) solution for use; specifically, adding deionized water to a three-necked round-bottom flask, slowly adding polyvinyl alcohol solid particles under stirring at room temperature, slowly stirring until there are no lumps, placing the beaker in an oil bath, heating to 60° C., soaking and slowly stirring for 30 min, so that the particles are fully expanded and elastic; then heating to 98° C., boiling, and slowly stirring for 30 min to prepare a 20 wt % PVA solution;

[0064] (2) 20 g of glass fiber was placed in acetone, ultrasonically dispersed for 30 minutes, and then soaked overnight to remove the surface impregnation material. After drying, the glass fiber was immersed in a mixture of concentrated sulfuric acid / hydrogen peroxide and stirred overnight to fully expose the silanol groups on the surface of the glass fiber. The glass fiber was washed, filtered, and dried for later use. In the mixture of concentrated sulfuric acid / hydrogen peroxide, the volume ratio of concentrated sulfuric acid to hydrogen peroxide was 7:3.

[0065] (3) The mass ratio of polyvinyl alcohol to pretreated glass fiber is 7:1. After ultrasonic mixing for 3 hours, the resulting solution is poured into a long strip mold and placed at -40°C for preliminary freezing for 2 hours. After being taken out and completely thawed, it is stretched and fixed with a stretching ratio of 300%. The stretched material is placed at -40°C again for two cycles of freeze-thaw, each time for 8 hours, and thawed at room temperature for 3 hours. After cyclic freeze-thaw, a polyvinyl alcohol / glass fiber composite material is obtained.

[0066] The polyvinyl alcohol / modified glass fiber composite materials prepared in Examples 1 to 3 were subjected to tensile tests, and the test results are shown in Tables 1 to 2. The test method is specifically as follows: in accordance with GB / T 1447-2005, an MTS Exceed E43 electronic universal testing machine (maximum test force 10 kN; product model: E43.104) was used to test the mechanical properties of the composite material sample; wherein the length of the sample was 13 cm, the thickness was 2 cm, and the speed of the loading head was 10 mm / min.

[0067] Table 1 shows the mechanical properties test results of the composite materials (parallel to the tensile direction)

[0068]

[0069] Table 2 shows the mechanical properties test results of the composite materials (perpendicular to the tensile direction)

[0070]

[0071]

[0072] By comparing the tensile strength of each composite material in the parallel direction and the vertical direction of Examples 1 to 3, it can be found that the modified glass fiber prepared by the present invention has good compatibility with the polyvinyl alcohol matrix material, and the active groups on the surface of the modified glass fiber form strong hydrogen bond interactions with the hydroxyl groups on the polyvinyl alcohol, thereby improving the interfacial bonding force and improving the mechanical properties of the composite material; by the substantial enhancement of the tensile strength in the vertical direction of Examples 1 to 3, it can be concluded that after the glass fiber is modified, its bonding strength with polyvinyl alcohol can be effectively enhanced, thereby enhancing the mechanical properties and toughness of the composite material, and the polyvinyl alcohol / modified glass fiber composite material containing three different hydrogen bonding effects can increase the tensile strength of the composite material by up to 300% compared with the polyvinyl alcohol matrix material without adding glass fiber. The present invention introduces active groups into the surface of the glass fiber by modification, and introduces them into the polyvinyl alcohol matrix material as a reinforcement, and through the hydrogen bond interaction between the active groups and PVA, the tensile strength and rigidity of the composite material can be effectively enhanced, that is, the active groups on the surface of the modified glass fiber form hydrogen bonds with the hydroxyl groups of PVA, thereby enhancing the mechanical properties of the composite material.

[0073] The transmittance of the composite materials prepared in Examples 1 to 3 was tested with reference to the standard GB / T 12010.8-2010. The transmittance of the samples was tested by a UV-visible spectrophotometer. The test results are shown in Table 3.

[0074] Table 3 is the test results of composite material transmittance

[0075]

[0076] By comparing the transmittance of the composite materials in Examples 1 to 3, it can be found that after the modified glass fiber is introduced into the polyvinyl alcohol matrix material, the transmittance of the composite material is significantly increased, indicating that after the modified glass fiber is added to the polyvinyl alcohol, the cross-linking structure inside the composite material is adjusted, and the significant increase in its transmittance reflects the formation of strong hydrogen bond interactions inside it.

[0077] The results of mechanical properties test show that compared with pure PVA, the tensile strength of polyvinyl alcohol / original glass fiber composite material is slightly enhanced, but much less than that of polyvinyl alcohol / modified glass fiber composite material; the results of transmittance test show that compared with pure PVA, the transmittance of polyvinyl alcohol / original glass fiber composite material is slightly enhanced, but much less than that of polyvinyl alcohol / modified glass fiber composite material. The above results prove that the glass fiber in polyvinyl alcohol / original glass fiber composite material is only used as a simple filler and fails to significantly improve the mechanical properties and transmittance of the composite material. There is a strong hydrogen bond interaction force inside the polyvinyl alcohol / modified glass fiber composite material, which leads to the adjustment of its internal cross-linking structure and the improvement of mechanical properties.

Claims

1. A polyvinyl alcohol / modified glass fiber composite material, characterized in that: The composite material is composed of a polyvinyl alcohol matrix and modified glass fibers bonded to the polyvinyl alcohol matrix through hydrogen bonding; the modified glass fibers are amino glass fibers, carboxyl glass fibers or hydroxylated glass fibers; The preparation method of the polyvinyl alcohol / modified glass fiber composite material comprises the following steps: (1) Preparing a polyvinyl alcohol solution; (2) Preparation of amino glass fiber, carboxylated glass fiber or hydroxylated glass fiber; The amino glass fiber is prepared by the following method: immersing the pretreated glass fiber in a toluene solution of an aminosilane coupling agent with a mass concentration of 10% to 20%, refluxing at 100 to 120° C. for 12 to 36 hours, and vacuum drying to obtain the amino glass fiber; The carboxylated glass fiber is prepared by the following method: the amino glass fiber is placed in N,N-dimethylacrylamide, after ultrasonic dispersion, it is transferred to an oil bath for stirring, succinic anhydride is added dropwise thereto while stirring, stirring is continued at 50-70°C for 12-36 hours, and the carboxylated glass fiber is obtained after vacuum drying; The hydroxylated glass fiber is prepared by the following method: the pretreated glass fiber is immersed in toluene, and after ultrasonic dispersion, KH560 hydrolyzate is added thereto, mixed and refluxed at 100-120°C for 3-5h, and then a boiling methanol and tetrafluoroboric acid mixed solution is added thereto, refluxed for 0.5-2h, then cooled to room temperature and concentrated ammonia water is added dropwise to adjust the solution to neutrality, and vacuum dried to obtain the hydroxylated glass fiber; Pretreatment of the glass fiber, specifically: placing the glass fiber in acetone, ultrasonically dispersing it, soaking it overnight to remove the surface impregnation material, drying it, and then soaking it in a concentrated sulfuric acid / hydrogen peroxide mixture and stirring it overnight to fully expose the silanol groups on the surface of the glass fiber, washing it, drying it, and then setting it aside; (3) The modified glass fiber is mixed with a polyvinyl alcohol solution and subjected to ultrasonic treatment. The resulting solution is poured into a mold and initially frozen at -20 to 40 °C for 2 to 4 h. After being taken out and completely thawed, the material is stretched and fixed. The stretched material is placed at -20 to 40 °C and subjected to freeze-thaw cycles for 2 to 4 times; each time the material is frozen for 8 to 12 h and thawed at room temperature for 1 to 3 h. After cyclic freeze-thaw cycles, a polyvinyl alcohol / modified glass fiber composite material is obtained.

2. The polyvinyl alcohol / modified glass fiber composite material according to claim 1, characterized in that: The mass ratio of polyvinyl alcohol matrix to modified glass fiber is 5~7:

1.

3. The polyvinyl alcohol / modified glass fiber composite material according to claim 1, characterized in that: The modified glass fiber has a length of 10-20 mm and a diameter of 40-50 μm.

4. The polyvinyl alcohol / modified glass fiber composite material according to claim 1, characterized in that: In step (1), the mass concentration of the polyvinyl alcohol solution is 10-20%.

5. The polyvinyl alcohol / modified glass fiber composite material according to claim 1, characterized in that: In step (3), the stretching ratio during stretching is 100% to 300%.