A non-woven fabric for toughening thermoplastic composite materials and a preparation method thereof

The polyaryletherketone nonwoven fabric prepared by electrospinning technology is inserted into the thermoplastic composite layer, solving the problem that the thermosetting resin system cannot improve the impact resistance of thermoplastic composite materials, significantly improving the compression strength after impact and being suitable for aviation heat Plastic composite material.

CN116163069BActive Publication Date: 2024-12-06DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211627787.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-12-06
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The existing non-woven fabrics are mainly suitable for thermosetting resin systems, and it is difficult to significantly improve the impact resistance of unmodified thermoplastic composite materials such as PEEK composite materials, especially the compression strength CAI value after impact is difficult to reach 300MPa.

Method used

The non-woven fabric is prepared by electrospinning technology by dissolving soluble carboxyl-containing polyaryletherketone resin in polar organic solvents, and inserting it between the layers of the thermoplastic composite material. The preform is formed by high temperature and high pressure to improve the composite material. impact toughness.

Benefits of technology

It significantly improves the post-impact compression strength of thermoplastic composite materials, improves the continuity and strength of non-woven fabrics, enhances the interlayer bonding force of composite materials, meets the performance requirements of thermoplastic composite materials for aviation, and improves production efficiency .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005078844940000011
    Figure FDA0005078844940000011
  • Figure FDA0005078844940000012
    Figure FDA0005078844940000012
  • Figure HDA0004004410040000011
    Figure HDA0004004410040000011
Patent Text Reader

Abstract

The present invention discloses a non-woven fabric for toughening thermoplastic composite materials and a preparation method thereof, and belongs to the field of electrostatic spinning technology. The preparation method comprises the following steps: a soluble polyaryletherketone resin is dissolved in a polar organic solvent, and a non-woven fabric is prepared by electrostatic spinning technology, wherein the thickness of the non-woven fabric is 5 to 30 μm and the fiber diameter is 0.5 to 5 μm. The non-woven fabric is arranged between layers of a multi-layer thermoplastic composite prepreg for toughening modification. During the composite material molding process, the non-woven fabric has a porous structure and will not hinder the longitudinal flow of the thermoplastic resin. The non-woven fabric can form a good combination with the resin, and even partially compatible, forming a toughening form of an interpenetrating network, greatly improving the interlayer bonding force, and thus improving the impact toughness of the composite material. The non-woven fabric prepared by the present invention can improve the post-impact compression strength of PEEK and PEKK resin-based composite materials, and meet the performance requirements of thermoplastic composite materials for aviation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a non-woven fabric for toughening a thermoplastic composite material and a preparation method thereof, and belongs to the technical field of electrostatic spinning. Background Art

[0002] Polyaryletherketone is a high-performance special engineering plastic with excellent thermal properties, mechanical properties, flame retardancy, low dielectric properties and impact resistance, etc. It is widely used in high-tech fields such as aerospace, transportation, and medical treatment. In addition, amorphous polyaryletherketone resin is soluble in organic solvents, which further expands the processing methods of polyaryletherketone and has broad application prospects.

[0003] Improving the impact toughness of composite materials is an important research direction for advanced composite materials. By making them tougher, the impact damage resistance and design allowable strain of composite materials can be effectively improved, and the weight reduction efficiency of composite materials can be improved. For RTM epoxy resin ZL2006100993819, thermoplastic film is laid between the layers of reinforced fabric to achieve the purpose of toughening, and the post-impact compressive strength CAI of the composite material is significantly improved. ZL201110362357.0 discloses a non-woven fabric for toughening composite materials, and the CAI value of the composite material is also significantly improved.

[0004] Existing commercial non-woven fabrics are all matched with thermosetting resin systems such as epoxy resin, and no research has been conducted on thermoplastic resin-based composite materials. The CAI of unmodified PEEK composite materials is difficult to reach 300MPa. Therefore, it is very necessary to improve the impact resistance of thermoplastic composite materials through interlayer modification. Summary of the invention

[0005] In order to solve the problems of the prior art, the present invention provides a non-woven fabric for toughening a thermoplastic composite material and a preparation method thereof, and the non-woven fabric is used to prepare the thermoplastic composite material.

[0006] A method for preparing a non-woven fabric for toughening a thermoplastic composite material, the steps of which are as follows:

[0007] (1) dissolving a soluble carboxyl-containing polyaryletherketone resin in a polar organic solvent to a solution mass concentration of 15 to 30%, stirring and dispersing the solution uniformly to obtain a clear and transparent spinning solution;

[0008] (2) The spinning solution of step (1) is placed in a syringe of an electrospinning device, the syringe needle is connected to the positive electrode of a high-voltage power supply, and the aluminum foil receiving plate is connected to the negative electrode of the high-voltage power supply. Spinning is performed under a certain ambient temperature and humidity, and a non-woven fabric is prepared on the aluminum foil receiving plate by electrospinning technology;

[0009] (3) Soaking the non-woven fabric obtained in step (2) in anhydrous ethanol for 10 to 60 minutes and drying it to finally obtain a polyaryletherketone non-woven fabric.

[0010] The carboxyl-containing polyaryletherketone resin has the following structure:

[0011] Where m:n=1~3:7~9, Ar can be selected as:

[0012] One of the above, the intrinsic viscosity of the resin is between 0.5 and 1.0 dL / g.

[0013] Based on the above technical scheme, preferably, in step (1), the polar organic solvent contains at least one or more of dioxane and DMF, DMAc, benzyl alcohol and 5-(dimethylamino)-2-methyl-5-oxopentanoic acid methyl ester (Polarclean), and the organic solvent is preferably a mixed solvent of dioxane and DMF or a mixed solvent of dioxane and benzyl alcohol, wherein the mass fraction of dioxane is 20-40%.

[0014] Based on the above technical solution, preferably, in step (2), the applied voltage is 10-25 kV, the syringe advancement speed is 1-4 mL / h, the ambient temperature is 30-60° C., and the humidity is <30%.

[0015] Based on the above technical solution, preferably, in step (3), the drying temperature is 80-120°C.

[0016] Based on the above technical solution, preferably, the polyaryletherketone nonwoven fabric has a thickness of 5 to 30 microns, a fiber diameter of 0.5 to 5 μm, and preferably a fiber diameter of 0.8 to 3 μm.

[0017] Thermoplastic composite material toughening non-woven fabric prepared by the above method.

[0018] The above-mentioned non-woven fabric for toughening thermoplastic composite materials is used in the preparation of thermoplastic composite materials. The polyaryletherketone non-woven fabric is inserted between two layers of thermoplastic composite prepreg to prepare a preform, and the preform is placed in a mold and kept warm for 20 to 40 minutes at a temperature of 320 to 360°C and a pressure of 5 to 10 MPa to prepare a thermoplastic composite material.

[0019] Based on the above technical scheme, preferably, the thermoplastic composite prepreg is prepared from a matrix resin and fibers, the matrix resin is a thermoplastic resin such as PEEK, PEKK, etc., and the melt index of the resin ranges from 20 to 80 g / 10min (380°C / 10kg); the fibers include carbon fibers, glass fibers, aramid fibers, etc.

[0020] Based on the above technical solution, preferably, the mass fraction of the polyaryletherketone resin in the composite material is 2-12%, the mass fraction of the thermoplastic resin is 25-35%, and the mass fraction of the fiber is 53-73%.

[0021] Beneficial effects of the present invention: The present invention provides a non-woven fabric for toughening thermoplastic composite materials and a preparation method thereof, which draws on the toughening mechanism of thermosetting resin composite materials to solve the impact toughness of thermoplastic composite materials. The use of a compound solvent solves the problems of easy clogging and discontinuity of needles in the preparation of phenolphthalein polyaryletherketone (PEK-C) non-woven fabrics, and the prepared non-woven fabrics are fluffy, easy to deform, and unable to be laid. The micron-level non-woven fabrics have good strength and are not deformed when torn, which can significantly improve the post-impact compression strength of thermoplastic composite materials. At the same time, the diameter reaches the micron level, which can greatly improve the production efficiency of electrostatic spinning equipment, which is conducive to industrial production. In the composite material molding process, the non-woven fabric has a porous structure and will not hinder the longitudinal flow of thermoplastic resin. The non-woven fabric can form a good combination with the resin, and even partially compatible, forming a toughening form of an interpenetrating network, greatly improving the interlayer bonding force, and then improving the impact toughness of the composite material. The non-woven fabric prepared by the present invention can improve the post-impact compression strength of PEEK and PEKK resin-based composite materials, and meet the performance requirements of thermoplastic composite materials for aviation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 PEK-C non-woven fabric prepared using traditional DMF as solvent.

[0023] Figure 2 This is the modified nonwoven fabric prepared in Example 1; the scale of the right figure is 1 μm. DETAILED DESCRIPTION

[0024] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0025] Example 1

[0026] The carboxyl-containing polyaryletherketone resin is dissolved in a mixed solvent of dioxane and DMF, the volume ratio of dioxane to DMF is 2:8, the mass concentration of the solution is 15%, and the mixture is evenly dispersed by stirring to obtain a clear and transparent spinning solution; the spinning solution is placed in a 10ml syringe of an electrospinning device, the syringe needle is connected to the positive electrode of a high-voltage power supply, and the aluminum foil receiving plate is connected to the negative electrode of the high-voltage power supply. A voltage of 15kV is applied, and spinning is performed at 30°C and 25% humidity. The propulsion speed is 2ml / h, and a non-woven fabric is obtained on the aluminum foil receiving plate. The obtained non-woven fabric is soaked in anhydrous ethanol for 10min, dried in a blast oven at 80°C, and finally a polyaryletherketone non-woven fabric is obtained.

[0027] Insert a polyaryletherketone nonwoven fabric with a thickness of 10μm and a fiber diameter of 2μm between two layers of PEEK / T700 carbon fiber composite prepreg to prepare a preform, place the preform in a mold, heat to 360℃ and hold the pressure at 10MPa for 30min to prepare a thermoplastic composite material, the melt index of PEEK is 40g / 10min (380℃ / 10kg). The mass fraction of polyaryletherketone resin in the composite material is 4%, the mass fraction of PEEK resin is 30%, and the mass fraction of carbon fiber is 66%. The post-impact compressive strength CAI of the composite material reaches 320MPa, and the CAI of unmodified PEEK / T700 is 280MPa.

[0028] The carboxyl-containing polyaryletherketone resin has the following structure:

[0029] m:n=1:9, the intrinsic viscosity of the resin is 0.7 dL / g.

[0030] Example 2

[0031] The carboxyl-containing polyaryletherketone resin is dissolved in a mixed solvent of dioxane and benzyl alcohol, the volume ratio of dioxane and benzyl alcohol is 3:7, the mass concentration of the solution is 20%, and the solution is stirred and dispersed evenly to obtain a clear and transparent spinning solution; the spinning solution is placed in a 10ml syringe of an electrospinning device, the syringe needle is connected to the positive electrode of a high-voltage power supply, the aluminum foil receiving plate is connected to the negative electrode of the high-voltage power supply, a voltage of 20kV is applied, spinning is performed at 40°C and 20% humidity, the propulsion speed is 4ml / h, and a non-woven fabric is obtained on the aluminum foil receiving plate. The obtained non-woven fabric is soaked in anhydrous ethanol for 20min, dried in a blast oven at 100°C, and finally a polyaryletherketone non-woven fabric is obtained.

[0032] A polyaryletherketone nonwoven fabric with a thickness of 20 μm and a fiber diameter of 1 μm was inserted between two layers of PEKK / T700 carbon fiber composite prepreg to prepare a preform, and the preform was placed in a mold, heated to 340°C and maintained at 5 MPa for 20 minutes to prepare a thermoplastic composite material. The melt index of PEKK is 52 g / 10 min (380°C / 10 kg). The mass fraction of polyaryletherketone resin in the composite material is 8%, the mass fraction of PEKK resin is 28%, and the mass fraction of carbon fiber is 64%. The post-impact compressive strength CAI of the composite material is 330 MPa, and the CAI of the unmodified PEKK / T700 carbon fiber composite material is 285 MPa.

[0033] The carboxyl-containing polyaryletherketone resin has the following structure:

[0034] m:n=2:8, the intrinsic viscosity of the resin is 0.5 dL / g.

Claims

1. Application of a nonwoven fabric for toughening a thermoplastic composite material in the preparation of a thermoplastic composite material, characterized in that: The preparation method of the nonwoven fabric comprises the following steps: (1) dissolving a carboxyl-containing polyaryletherketone resin in a polar organic solvent, stirring and dispersing the mixture uniformly, and obtaining a spinning solution; wherein the mass concentration of the carboxyl-containing polyaryletherketone resin in the spinning solution is 15 to 30%; (2) placing the spinning solution of step (1) in a syringe of an electrospinning device, connecting the syringe needle to the positive electrode of a high-voltage power supply, connecting an aluminum foil receiving plate to the negative electrode of the high-voltage power supply, spinning under a certain ambient temperature and humidity, and obtaining a non-woven fabric on the aluminum foil receiving plate; (3) soaking the non-woven fabric obtained in step (2) in anhydrous ethanol for 10 to 60 minutes, and drying to finally obtain a polyaryletherketone non-woven fabric; The carboxyl-containing polyaryletherketone resin has the following structure: Where Ar is: One of the above, wherein the intrinsic viscosity of the resin is 0.5 to 1.0 dL / g.

2. The use according to claim 1, characterized in that: In step (1), the polar organic solvent contains at least one or more of dioxane, DMF, DMAc, benzyl alcohol and 5-(dimethylamino)-2-methyl-5-oxopentanoic acid methyl ester.

3. The use according to claim 1, characterized in that: In step (2), the applied voltage is 10-25 kV, the syringe advancement speed is 1-4 mL / h, the ambient temperature is 30-60° C., and the humidity is less than 30%.

4. The use according to claim 1, characterized in that: In step (3), the drying temperature is 80-120°C.

5. The use according to claim 1, characterized in that: The polyaryletherketone nonwoven fabric has a thickness of 5 to 30 micrometers and a fiber diameter of 0.5 to 5 micrometers.

6. The use according to claim 1, characterized in that: The nonwoven fabric is inserted between two layers of thermoplastic composite prepreg, and the thermoplastic composite is prepared by high-temperature molding.

7. The use according to claim 1, characterized in that: The matrix resin of the thermoplastic composite material prepreg is PEEK or PEKK, and the melt index of the resin is 20-80 g / 10 min (380° C. / 10 kg).