By using composite catalytic materials in the VOCs oxidation process, including framework heteroatom molecular sieves and dispersed metal elements, efficient VOCs oxidation under mild conditions is achieved, solving the problems of low catalytic oxidation efficiency and high by-products in the existing technology. Improved catalytic activity and complete combustion selectivity.
Patent Information
- Application Number
- CN202111424549.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The existing technology has low catalytic oxidation efficiency and many by-products in the treatment of low-concentration VOCs, making it difficult to achieve complete oxidation, and it is difficult for a single technology to handle the diversity and complexity of VOCs.
Using composite catalytic materials, including framework heteroatom molecular sieves and metal elements M dispersed in the molecular sieve, efficient oxidation of VOCs is achieved under mild conditions through oxygen oxidation reaction, and the synergistic catalytic effect of heteroatoms and metal elements is used to improve catalytic activity.
It achieves high conversion rate of VOCs gas and improved selectivity of complete combustion products under mild reaction conditions, which has high industrial application value.
Smart Images

Figure CN116173723B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of organic chemical industry, and in particular, to a VOCs gas oxidation method. Background Art
[0002] According to the definition of the World Health Organization (WHO), VOCs (volatile organic compounds) are various organic compounds with a boiling point of 50°C to 260°C at room temperature. In my country, VOCs refer to organic compounds with a saturated vapor pressure greater than 70Pa at room temperature and a boiling point below 260°C at normal pressure, or all organic compounds with a vapor pressure greater than or equal to 10Pa and volatility at 20°C. They are usually divided into several major categories, such as non-methane hydrocarbons (referred to as NMHCs), oxygen-containing organic compounds, halogenated hydrocarbons, nitrogen-containing organic compounds, and sulfur-containing organic compounds. VOCs participate in the formation of ozone and secondary aerosols in the atmospheric environment, and have an important impact on regional atmospheric ozone pollution and PM2.5 pollution. Most VOCs have a special unpleasant odor and are toxic, irritating, teratogenic and carcinogenic. In particular, benzene, toluene and formaldehyde can cause great harm to human health. VOCs are important precursors to urban haze and photochemical smog, and are mainly derived from coal chemical industry, petrochemical industry, fuel coating manufacturing, solvent manufacturing and use, and other processes.
[0003] Low-temperature catalytic oxidation is highly efficient and economical, and has been widely studied in the field of research and application. Low-temperature catalytic oxidation mainly includes regenerative catalytic oxidation, photocatalytic oxidation and catalytic mixed treatment. With the continuous development and optimization of industrial processes, most VOCs pollution sources tend to emit low-concentration VOCs. In this case, traditional technologies cannot achieve the ideal VOCs treatment effect, and there are multiple VOCs in each industrial pollution source. Therefore, the types of VOCs involved will compete with each other for catalytic oxidation; and then incomplete oxidation leads to low removal rate and by-products. Due to the diversity and complexity of VOCs, it is unrealistic to remove them all by a single technology. At present, the technology combining catalysis with adsorption concentration, ozone oxidation, etc. is more effective and suitable. However, this technology still relies on the high efficiency of the catalytic process.
[0004] Therefore, it is crucial to develop an excellent catalytic system for the oxygen oxidation process of VOCs, among which the development of heterogeneous catalysts with high catalytic activity in the oxygen oxidation process of VOCs is key. Summary of the invention
[0005] The purpose of the present disclosure is to provide a VOCs gas oxidation method, which can achieve efficient oxidation of VOCs gas under heterogeneous composite catalytic materials and oxygen conditions, and obtain a high conversion rate of VOCs gas under mild reaction conditions, and has high industrial application value.
[0006] In order to achieve the above-mentioned purpose, the present disclosure provides a VOCs gas oxidation method, comprising: in the presence of oxygen, bringing the VOCs gas into contact with a catalyst for an oxidation reaction; the catalyst is a composite catalytic material, and the composite catalytic material comprises a skeleton heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the skeleton heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the skeleton of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium.
[0007] Optionally, the conditions for the oxidation reaction include: the volume ratio of oxygen to VOCs gas is 1 to 10:1, preferably 4 to 10:1; the gas volume space velocity of VOCs is 3000 to 6000 h -1 , preferably 3000~5000h -1 ; The reaction temperature is 150 to 300°C, preferably 150 to 250°C; the reaction time is 1 to 48h, preferably 2 to 24h;
[0008] Optionally, the VOCs are one or more selected from non-methane hydrocarbons, oxygen-containing organic compounds, halogenated hydrocarbon compounds, nitrogen-containing organic compounds and sulfur-containing organic compounds;
[0009] Preferably, the non-methane hydrocarbon is selected from one or more of ethane, ethylene, acetylene, benzene, xylene, styrene and naphthalene;
[0010] The oxygen-containing organic compound is selected from one or more of methyl tert-butyl ether, formaldehyde, benzaldehyde and phenol;
[0011] The halogenated hydrocarbon compound is selected from one or more of trichloroethylene, chloroform and trichloroethane;
[0012] The nitrogen-containing organic compound is selected from one or more of diisocyanate compounds having 1 to 16 carbon atoms, diisocyanatolyl compounds having 1 to 16 carbon atoms, amine compounds having 1 to 16 carbon atoms, and amide compounds having 1 to 16 carbon atoms; preferably, the nitrogen-containing organic compound is selected from one or more of aniline, propionamide, and toluene diisocyanate;
[0013] The sulfur-containing organic compound is selected from one or more of sulfide compounds having 2 to 16 carbon atoms, thiol compounds having 1 to 16 carbon atoms, and thiophene compounds having 4 to 16 carbon atoms; preferably, the sulfur-containing organic compound is selected from one or more of benzothiophene, methyl mercaptan, and dimethyl sulfide;
[0014] Optionally, the reactor for the oxidation reaction is selected from any one of a tank reactor, a fixed bed reactor, a moving bed reactor, a suspended bed reactor or a slurry bed reactor.
[0015] Optionally, the composite catalytic material has the following UV-Vis characteristics:
[0016] The peak area of the spectrum peak in the wavelength range of 460 to 540 nm obtained by the peak separation result of the wavelength of 460 to 740 nm in the UV-Vis spectrum of the composite catalyst material is recorded as A1, and the total peak area in the wavelength range of 460 to 740 nm in the UV-Vis spectrum of the composite catalyst material is recorded as A2.
[0017] A0 defined by the following formula (1) is any value between 10% and 20%;
[0018] A0=A1 / A2 Formula (1);
[0019] Preferably, the A0 is any value between 10 and 18%.
[0020] Optionally, the framework heteroatom molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0021] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0022] Optionally, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1, preferably (0.001-0.043):1;
[0023] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.001-0.16):1.
[0024] Optionally, the BET specific surface area of the composite catalytic material is 360 to 800 m 2 / g, the total pore volume is 0.30-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.18-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-4.5nm.
[0025] Optionally, the composite catalytic material is prepared by a preparation method comprising the following steps:
[0026] S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture;
[0027] S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments;
[0028] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.
[0029] Optionally, in step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005-1): (0.001-0.05): (10-80): (0.002-0.2): (0.015-0.4); preferably 1: (0.005-1): (0.002-0.043): (10-80): (0.001-0.165): (0.015-0.3); the molar ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01-3): 1, preferably (0.01-2): 1.
[0030] Optionally, step S1 includes the following steps:
[0031] a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution;
[0032] b. adding the dendritic macromolecule to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material;
[0033] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;
[0034] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
[0035] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0036] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0037]
[0038] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0039] Optionally, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0040] wherein R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from one of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group and a tert-butyl group;
[0041] Further preferably, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0042] The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0043] The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0044] Optionally, in step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain the hydrolysis solution;
[0045] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0046] Optionally, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one selected from chlorides, nitrates and sulfates of heteroatom element Q; the inorganic skeleton heteroatom precursor is an organic acid ester containing heteroatom element Q, selected from at least one of the structures represented by the following formula (C):
[0047]
[0048] wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R5, R6, R7 and R8 are independently selected from a straight-chain alkyl group having 2 to 4 carbon atoms and a branched-chain alkyl group having 2 to 4 carbon atoms;
[0049] Optionally, R5, R6, R7 and R8 are each independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl; preferably, each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl;
[0050] Preferably, when the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is boron, the skeleton heteroatom precursor is selected from one or more of boric acid and borate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is aluminum, the skeleton heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; when the skeleton heteroatom is phosphorus, the skeleton heteroatom precursor is selected from one or more of orthophosphoric acid, triethyl phosphoric acid and metaphosphate; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.
[0051] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal M precursor is a water-soluble inorganic salt of the metal element M;
[0052] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0053] Preferably, the metal M precursor is an aqueous solution of the metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0054] Optionally, in step S1, the dendritic macromolecule is selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules;
[0055] Preferably, the polyamidoamine macromolecule is selected from one or more of the 2nd generation PAMAM with an ethylenediamine core, the 3rd generation PAMAM with an ethylenediamine core, and the 4th generation PAMAM with an ethylenediamine core;
[0056] The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone;
[0057] Preferably, the dendrimer has a weight average molecular weight of 4,000 to 85,000, a viscosity at 30° C. of 0.025 to 0.045 dL / g, and a degree of branching of 4,000 to 18,000.
[0058] Optionally, in step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the carbon number of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer from 1 to 18, and the carbon number of the aromatic group is any integer from 6 to 18;
[0059] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0060] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;
[0061] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0062] Through the above technical scheme, the present disclosure provides a VOCs gas oxidation method, which uses oxygen as an oxidant to carry out a heterogeneous oxidation reaction, and uses a composite catalytic material including a framework heteroatom molecular sieve and metal elements dispersed in the crystals of the molecular sieve as a catalyst. The heteroatom framework molecular sieve of the composite catalytic material has a multi-level pore structure and a large specific surface area, pore volume and reaction activity; and the metal oxide nanoparticles have a uniform particle size and are evenly dispersed in the crystals of the multi-level pore heteroatom framework molecular sieve (for example, in the mesoporous channels), the heteroatom Q in the framework and the metal element M nanoparticles outside the framework have a synergistic catalytic effect, further improving the catalytic activity of the composite catalytic material in the VOCs gas oxidation reaction; under mild reaction conditions, efficient oxidation of VOCs gas can be achieved, the VOCs gas conversion rate and the selectivity of complete combustion products are improved, and the composite catalytic material has extremely high industrial application value.
[0063] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0065] Figure 1 This is the UV-Vis spectrum of the product obtained in Preparation Example 1.
[0066] Figure 2 This is a peak analysis diagram of the UV-Vis spectrum of the product prepared in Preparation Example 1.
[0067] Figure 3 This is the XRD spectrum of the product prepared in Preparation Example 1.
[0068] Figure 4 This is the SEM spectrum of the product prepared in Preparation Example 1. DETAILED DESCRIPTION
[0069] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0070] The present disclosure provides a VOCs gas oxidation method, comprising the following steps: in the presence of oxygen, bringing the VOCs gas into contact with a catalyst for oxidation reaction; the catalyst is a composite catalytic material, the composite catalytic material comprising a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium.
[0071] The method provided by the present invention uses oxygen as an oxidant and a composite catalytic material including a framework heteroatom molecular sieve and metal elements dispersed in the crystals of the molecular sieve as a catalyst, so that efficient oxidation of VOCs gas can be achieved under low temperature conditions, the VOCs gas conversion rate and the selectivity of complete combustion products can be improved, and the industrial application value is extremely high; wherein the heteroatom Q in the framework of the composite catalytic material and the metal element M nanoparticles outside the framework have a synergistic catalytic effect, further improving the catalytic activity of the composite catalytic material in the VOCs gas oxidation reaction.
[0072] In one embodiment, the conditions of the oxidation reaction include: the volume ratio of oxygen to VOCs gas is 1 to 10:1, preferably 4 to 10:1; the gas volume space velocity (GHSV) of the VOCs is 3000 to 6000 h -1 , preferably 3000~5000h -1 , where gas volume space velocity (GHSV) = standard volume flow rate into the reactor (m 3 / h) / catalyst volume of reactor (m 3 ); the reaction temperature is 150-300°C, preferably 150-250°C; the reaction time is 1-48h, preferably 2-24h.
[0073] In one embodiment, the VOCs are one or more selected from non-methane hydrocarbons, oxygen-containing organic compounds, halogenated hydrocarbon compounds, nitrogen-containing organic compounds and sulfur-containing organic compounds.
[0074] In a specific embodiment, the non-methane hydrocarbon is selected from one or more of ethane, ethylene, acetylene, benzene, xylene, styrene and naphthalene, and its complete combustion product includes carbon dioxide;
[0075] The oxygen-containing organic compound is selected from one or more of methyl tert-butyl ether, formaldehyde, benzaldehyde and phenol, and its complete combustion product includes carbon dioxide;
[0076] The halogenated hydrocarbon compound is selected from one or more of trichloroethylene, chloroform and trichloroethane, and its complete combustion products include carbon dioxide and hydrogen halide;
[0077] The nitrogen-containing organic compound is selected from one or more of diisocyanate compounds having 1 to 16 carbon atoms, diisocyanatolyl compounds having 1 to 16 carbon atoms, amine compounds having 1 to 16 carbon atoms, and amide compounds having 1 to 16 carbon atoms; preferably, the nitrogen-containing organic compound is selected from one or more of aniline, propionamide, and toluene diisocyanate, and its complete combustion products include carbon dioxide and nitrogen;
[0078] The sulfur-containing organic compound is selected from one or more of sulfide compounds with carbon atoms of 2 to 16, thiol compounds with carbon atoms of 1 to 16, and thiophene compounds with carbon atoms of 4 to 16; preferably, the sulfur-containing organic compound is selected from one or more of benzothiophene, methyl mercaptan and dimethyl sulfide, and its complete combustion products include carbon dioxide and hydrogen sulfide.
[0079] The complete combustion products of the VOCs gas described in the present disclosure are based on substances well known to those skilled in the art.
[0080] In a specific embodiment, the reactor for the oxidation reaction is selected from any one of a tank reactor, a fixed bed reactor, a moving bed reactor, a suspended bed reactor or a slurry bed reactor.
[0081] In one embodiment, the composite catalytic material has the following UV-Vis characteristics:
[0082] In the peak separation result of the wavelength of 460 to 740 nm in the UV-Vis spectrum of the composite catalytic material, the peak area of the spectrum peak in the wavelength range of 460 to 540 nm is recorded as A1, and the total peak area in the wavelength range of 460 to 740 nm in the UV-Vis spectrum of the composite catalytic material is recorded as A2.
[0083] A0 defined by the following formula (1) is any value between 10% and 20%;
[0084] A0=A1 / A2 Formula (1).
[0085] The present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves, wherein the molecular sieve of the composite catalytic material has a multi-level pore structure and a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore heteroatom framework molecular sieve. There is an obvious interaction between the metal elements of the metal oxide particles and the heteroatoms in the framework. After the heteroatoms are introduced into the molecular sieve framework, the two metal sites in the composite catalytic material can play a synergistic catalytic role, effectively improving the catalytic activity of the composite catalytic material for macromolecular substrates. In addition, in the present disclosure, by controlling A0 to be any value between 10 and 20% (i.e., controlling the ratio of the peak area of the spectrum peak in the wavelength range of 460 to 540 nm to the total peak area in the wavelength range of 460 to 740 nm), the active components in the composite catalytic material can be more and the catalytic effect can be better.
[0086] The inventors of the present disclosure surprisingly discovered through a large number of experiments that heteroatom precursors, metal M precursors, dendritic macromolecules and silanization agents (containing at least one coordination group complexed with the metal element M) are introduced into the reaction raw materials for crystallization synthesis of molecular sieves, and after hydrothermal crystallization and calcination treatments, heteroatoms can be introduced into the molecular sieve framework, and the skeleton heteroatom molecular sieve of the composite catalytic material obtained has a multi-level pore structure (micropores and mesopores) and a large specific surface area and pore volume, the metal oxide nanoparticles have a high uniformity in particle size and can be evenly dispersed in the pores of the skeleton heteroatom molecular sieve, and a certain amount of metal M nanoparticles will also exist on the surface of the pores; the heteroatom metal sites on the molecular sieve framework and the metal sites (nanoparticles) of the metal element M in the pores can also play a synergistic catalytic effect, further improving the catalytic activity in the heterogeneous low-temperature oxidation reaction of VOCs gas.
[0087] Furthermore, the inventors also found that for the peak separation results of the 460-740nm wavelength in the UV-Vis spectrum of the obtained composite catalytic material, as the proportion of the peak area (A1) of the spectrum peak in the wavelength range of 460-540nm to the total peak area (A2) in the wavelength range of 460-740nm increases, the catalytic performance of the composite catalytic material shows a downward trend, and when the proportion of the peak area (A1) of the spectrum peak in the wavelength range of 460-540nm to the total peak area (A2) in the wavelength range of 460-740nm (i.e. A0) is controlled to any value between 10 and 20%, the composite catalytic material exhibits ideal catalytic activity in the heterogeneous low-temperature oxidation reaction of VOCs gas.
[0088] In the present disclosure, the peak separation of UV-Vis spectrum can be performed using conventional peak separation methods and software in the art.
[0089] In a preferred embodiment, A0 is any value between 10% and 18%. In this embodiment, the composite catalytic material has a higher catalytic activity.
[0090] In one embodiment, the skeleton heteroatom molecular sieve in the composite catalytic material is one or more of MFI structure molecular sieve (such as S-1), MEL structure molecular sieve (such as S-2), BEA structure molecular sieve (such as Beta), MWW structure molecular sieve (such as MCM-22), two-dimensional hexagonal structure molecular sieve (such as MCM-41, SBA-15), MOR structure molecular sieve (such as MOR), TUN structure molecular sieve (such as TUN) and silicon molecular sieves of other structures (such as ZSM-48, MCM-48); preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve, such as the silicon molecular sieve is one of S-1, S-2 and Beta; further preferably, it is an MFI structure molecular sieve, such as S-1.
[0091] In one embodiment, the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0092] In one embodiment, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1, preferably (0.001-0.043):1;
[0093] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.001-0.16):1.
[0094] In one embodiment, the BET specific surface area of the composite catalytic material is 360 to 800 m 2 / g, preferably 370 to 690 m 2 / g, the total pore volume is 0.3-0.65mL / g, preferably 0.33-0.61mL / g, the micropore volume is 0.1-0.19mL / g, preferably 0.12-0.18mL / g, the mesopore volume is 0.18-0.46mL / g, preferably 0.21-0.44mL / g, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-4.5nm, preferably 1.8-4.4nm; the composite catalytic material in the present disclosure has a multi-level pore structure, which is beneficial to catalyzing reaction substrates of different sizes.
[0095] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising the following steps:
[0096] S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture;
[0097] S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatment;
[0098] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.
[0099] The present disclosure introduces heteroatom precursors into the reaction mixture for synthesizing molecular sieves, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present disclosure also introduces metal element precursors, dendritic macromolecules and silanization agents into the reaction mixture. On the one hand, metal ions are complexed with groups such as amine groups contained in the dendritic macromolecules to achieve the effect of dispersing and stabilizing metals; at the same time, at least one coordination group (such as amine groups, thiol groups, oxygen-containing coordination groups, etc.) carried by the silanization agent can also be complexed with metal ions to achieve the effect of fixing and dispersing metals, so that the metal oxide nanoparticles in the molecular sieve channels obtained after hydrothermal crystallization and calcination have high dispersion; on the other hand, the alkyl chain of the silanization agent also ensures the realization of the molecular sieve support layer expansion effect of the synthesized composite catalytic material, and the molecular volume of the dendritic macromolecule is very large, which can play a good role in supporting layer isolation during the crystallization of the molecular sieve. So that a skeleton heteroatom molecular sieve with a multi-level pore structure is finally prepared, and the metal M oxide nanoparticles can also be evenly dispersed in the mesoporous channels of the multi-level pore skeleton heteroatom molecular sieve.
[0100] In one embodiment, in step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005-1): (0.001-0.05): (10-80): (0.002-0.2): (0.015-0.4); preferably 1: (0.005-1): (0.002-0.043): (10-80): (0.001-0.165): (0.015-0.3); the molar ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01-3): 1, preferably (0.01-2): 1.
[0101] Specifically, the water used in step S1 can be water commonly used in synthesizing molecular sieves. In order to avoid the introduction of heteroatoms, deionized water is preferred.
[0102] In a preferred embodiment, step S1 comprises the following steps:
[0103] a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution;
[0104] b. adding the dendritic macromolecule to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material;
[0105] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;
[0106] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
[0107] In one embodiment, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0108] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0109]
[0110] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
[0111] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0112] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.
[0113] In a further preferred embodiment, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0114] Wherein R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0115] In a preferred embodiment, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0116] In another preferred embodiment, the molecular sieve in the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0117] In another preferred embodiment, the molecular sieve in the composite catalyst material is a Beta molecular sieve, and the template is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0118] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution;
[0119] The conditions for the hydrolysis and alcohol removal treatment include: stirring hydrolysis at 0-95°C for 2-10 hours; preferably stirring hydrolysis at 50-95°C for 2-8 hours; wherein the hydrolysis and alcohol removal treatment makes the mass content of alcohol produced by hydrolysis of the organosilicon source in the hydrolysis solution less than 10 ppm.
[0120] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal element (such as a compound containing the metal element and / or a metal element) can achieve the purpose of the present disclosure.
[0121] In one embodiment, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one of a chloride, a nitrate or a sulfate of a heteroatom element; the inorganic skeleton heteroatom precursor is an organic acid ester containing a heteroatom element, selected from at least one of the structures represented by the following formula (C):
[0122]
[0123] wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R5, R6, R7 and R8 are independently selected from a straight-chain alkyl group having 2 to 4 carbon atoms and a branched-chain alkyl group having 2 to 4 carbon atoms;
[0124] Optionally, R5, R6, R7 and R8 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl; preferably, they are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
[0125] In an optional embodiment, the skeleton heteroatom is titanium, and the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; in an optional embodiment, the skeleton heteroatom is boron, and the skeleton heteroatom precursor is selected from one or more of boric acid and borate; in an optional embodiment, the skeleton heteroatom is tin, and the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide. In one optional embodiment, the framework heteroatom is aluminum, and the framework heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; in one optional embodiment, the framework heteroatom is phosphorus, and the framework heteroatom precursor is selected from one or more of orthophosphoric acid, triethylphosphoric acid and metaphosphate; in one optional embodiment, the framework heteroatom is germanium, and the framework heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide (such as ethanol germanium, isopropoxide germanium), germanium chloride and sodium germanate.
[0126] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal M precursor is a water-soluble inorganic salt of the metal element M;
[0127] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0128] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0129] In one embodiment, in step S1, the dendritic macromolecule is selected from one or more of polyamide-amine macromolecules (PAMAM) and polyarylether macromolecules;.
[0130] In a preferred embodiment, the polyamide-amine macromolecule is selected from one or more of the 2nd generation PAMAM with an ethylenediamine core, the 3rd generation PAMAM with an ethylenediamine core, and the 4th generation PAMAM with an ethylenediamine core;
[0131] The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone;
[0132] Preferably, the weight average molecular weight of the dendritic macromolecule is 4000-85000, the viscosity at 30°C is 0.025-0.045 dL / g, and the kinematic viscosity is 10-10000 mm 2 / s, and the degree of branching is 4000-18000 (relative molecular weight, measured in Mw).
[0133] The dendrimers used in the present disclosure can be purchased from any known channels, or prepared according to any disclosed preparation method.
[0134] In one embodiment, in step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer in the range of 1 to 18, preferably any integer in the range of 1 to 12; the number of carbon atoms of the aromatic group can be any integer in the range of 6 to 18, preferably any integer in the range of 6 to 12.
[0135] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0136] In the present disclosure, different silanization agents can be selected for different metal elements M. For example, when the metal element M is Co, the silanization agent is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; when the metal element M is Au or Pt, the silanization agent is at least one of 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.
[0137] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.
[0138] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.
[0139] In the present disclosure, the UV-visible diffuse reflectance spectrum (UV-vis) of the sample solid was measured on a SHIMADZU UV-3100 UV-visible spectrometer in the test range of 400 to 4000 cm -1 .
[0140] The X-ray diffraction (XRD) crystal phase diagram of the sample was measured on a Siemens D5005 X-ray diffractometer, the radiation source was Kα (Cu), and the test range 2θ was 0.5-70°.
[0141] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.
[0142] The average particle size of the metal nanoparticles in the molecular sieve of the sample was obtained by HR-TEM measurement.
[0143] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0144] In the following examples, among the dendritic macromolecules used, PAMAM is a polyamide-amine type dendritic macromolecule purchased from Inokai, wherein PAMAM (ethylenediamine core, 2nd generation) has a molecular weight of 9858, an intrinsic viscosity of 0.037 dL / g at 30°C, and a degree of branching of 4300 (Mw); PAMAM (ethylenediamine core, 3rd generation) has a molecular weight of 9858, an intrinsic viscosity of 0.035 dL / g at 30°C, and a degree of branching of 5200 (Mw); PAMAM (ethylenediamine core, 4th generation) has a molecular weight of 26000, an intrinsic viscosity of 0.031 dL / g at 30°C, and a degree of branching of 16000 (Mw); polyarylether macromolecules purchased from Inokai, polyarylether nitrile molecular weight of 83000. The weight average molecular weight of the dendritic macromolecules in the present disclosure is obtained by Ubbelohde viscometer and conventional methods; the degree of branching is obtained by reagent labels. The intrinsic viscosity is measured by an Ubbelohde viscometer using a conventional method.
[0145] The cobalt nitrate used in the following examples of the present disclosure is all cobalt nitrate hexahydrate.
[0146] Preparation Example 1
[0147] (1) 1.6 g of 25.05 wt% tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol), 0.17 g of tetrabutyl titanate (0.0005 mol) and 9 g (0.5 mol) of water were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 80° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;
[0148] (2) 0.3 g of cobalt nitrate hexahydrate (0.001 mol) and 1.8 g (0.1 mol) of water were stirred evenly, and then 0.06 g of PAMAM (ethylenediamine core, 2nd generation) was added, and the aqueous solution of the metal was mixed with the hydrolyzed solution of silicon obtained in step (1);
[0149] (3) adding 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) to the mixture of step (2) and stirring for 0.5 hour;
[0150] (4) The mixture obtained in step (3) was transferred to a stainless steel closed reactor and crystallized at a constant temperature of 170°C for 28 hours to obtain a sample. The obtained sample was filtered, washed, dried at 120°C for 6 hours, and then calcined at 600°C in a muffle furnace for 6 hours to obtain a metal nanoparticle and molecular sieve composite catalytic material product, which was recorded as catalyst A1.
[0151] The UV-Vis spectrum of A1 is as follows Figure 1 As shown, Figure 1 The peak near 220nm in the spectrum represents titanium species; the UV-Vis peak analysis is shown in Figure 2 shown. Figure 2 The peaks in the range of 460 to 740 nm indicate that there is an interaction between the Co species and the Si skeleton. The peak at 520 nm represents the species inside the cobalt oxide nanoparticles, the peak at 590 nm represents the species at the interface between the cobalt oxide nanoparticles and the silicon skeleton, and the peak at 660 nm represents the species on the surface of the cobalt oxide nanoparticles (active centers). The XRD spectrum of A1 is shown in Figure 2. Figure 3 As shown in Figure 2, XRD analysis shows that it has an MFI structure. The SEM spectrum of A1 is shown in Figure 2. Figure 4 As shown, it can be seen that the products have regular shapes and uniform sizes.
[0152] The BET specific surface area, total pore volume, micropore volume and mesopore volume of product A1, as well as the average particle size of the metal nanoparticles contained therein are listed in Table 2.
[0153] Preparation Comparative Example 1
[0154] The product was prepared according to the method of Preparation Example 1, except that no silanization agent was added. The obtained product was recorded as DA1.
[0155] Preparation Comparative Example 2
[0156] 0.03 g of cobalt nitrate hexahydrate and 0.18 g of water were stirred evenly to obtain an aqueous solution of the metal. Then 10.2 g of alumina carrier (purchased from Innochem, product number A17263) was added, stirred for 4 h, and the solvent was evaporated. The solid was collected and dried at 110 ° C for 6 hours, and then calcined at 550 ° C in a muffle furnace for 6 hours. The obtained product was recorded as DA2.
[0157] Preparation Comparative Example 3
[0158] 0.03 g of cobalt nitrate hexahydrate and 0.18 g of water were stirred evenly to obtain a metal aqueous solution. Then 6 g of titanium silicon MFI molecular sieve carrier was added, stirred for 4 hours, and the solvent was evaporated. The solid was collected and dried at 110°C for 6 hours, and then calcined at 550°C in a muffle furnace for 6 hours. The obtained product was recorded as DA3.
[0159] The titanium silicate MFI molecular sieve carrier refers to the preparation example 1, and the difference from the preparation example 1 is that step (2) is not performed, that is, cobalt nitrate hexahydrate and dendrimer macromolecules are not added in the molecular sieve synthesis, and the rest of the process is the same as the preparation example 1.
[0160] Preparation Examples 2 to 9
[0161] The corresponding products A2 to A9 were prepared according to the method of Preparation Example 1, and their proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1.
[0162] Preparation Example 10
[0163] The cobalt-containing multi-level porous β molecular sieve was prepared by referring to the method of Preparation Example 1, changing the ratio and template agent, and using tetraethylammonium hydroxide (TEAOH) as the template agent. The obtained product was recorded as A10. The ratio, synthesis conditions and results are shown in Table 1.
[0164] Preparation Example 11
[0165] The cobalt-containing multi-level porous MEL molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent, and using tetrabutylammonium hydroxide (TBAOH) as the template agent. The obtained product was recorded as A11. The ratio, synthesis conditions and results are shown in Table 1.
[0166] Preparation Example 12
[0167] The cobalt-containing multi-level porous MFI molecular sieve was prepared by referring to the method of Example 1. The proportions, synthesis conditions and results are shown in Table 1. The obtained product is recorded as A12. The hydrothermal crystallization temperature is 120°C and the hydrothermal crystallization time is 6 days; the calcination temperature is 870°C and the calcination time is 9 hours. The proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations are referred to Example 1.
[0168] The average particle size of the metal nanoparticles in the molecular sieves of the products obtained in the above examples and comparative examples, the BET specific surface area, the total pore volume, the micropore volume and the mesopore volume of the products are listed in Table 2.
[0169] Table 1
[0170]
[0171]
[0172] In m / 10×c*, m represents the mass of the dendrimer and c represents the amount of the silicon source in terms of SiO2.
[0173] In Table 1, TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane). The reagents used in the present disclosure can be obtained through conventional purchasing channels.
[0174] Table 2
[0175]
[0176]
[0177] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0178] According to Table 2, compared with DA-1 (without the addition of silanization agent), the composite catalytic materials A-1 to A-12 provided in the present disclosure have higher mesopore volumes, indicating that the method provided in the present disclosure can effectively expand the pores of the molecular sieve.
[0179] Compared with DA-1 to DA-3, the composite catalytic materials A-1 to A-12 provided in the present invention can simultaneously have a large mesopore volume, a large specific surface area and a smaller metal nanoparticle size, indicating that the metal nanoparticles in the composite catalytic materials obtained in the present invention have a lower degree of aggregation and a higher degree of dispersion.
[0180] Reaction Example 1
[0181] Used to illustrate the reaction effect of the composite catalytic material obtained by the method provided by the present invention for oxygen oxidation of VOCs.
[0182] The catalyst prepared in the above examples and comparative examples was used to catalyze the oxidation of VOCs (simulated by a molar ratio of toluene and methyl tert-butyl ether of 1:1, both of which were 500 ppm) by oxygen. Oxygen (using N2 as the balance gas, the volume ratio of oxygen to N2 was 1:4, and the total flow rate of the mixed gas was 50 mL / min) and VOCs were introduced into the reactor at a volume ratio of 5:1, and contacted with 0.5 g of the catalyst in a fixed bed reactor at a temperature of 200°C for 24 hours. The gas space velocity (GHSV) of VOCs was 5000 h -1 , space velocity = standard volume flow rate into the reactor (m 3 / h) / catalyst volume of reactor (m 3 ).
[0183] The obtained products were measured for distribution of each product on an Agilent 6890N chromatograph using an HP-5 capillary column (30 m×0.25 mm). The results are listed in Table 3 below.
[0184] VOCs conversion rate (%) = the number of moles of VOCs participating in the reaction / the number of moles of VOCs added×100%.
[0185] Selectivity of complete combustion products (%) = number of moles of complete combustion products / number of moles of VOCs participating in the reaction × 100%.
[0186] The number of moles of VOCs involved in the reaction = the number of moles of VOCs fed - the number of moles of VOCs remaining in the resulting reaction mixture.
[0187] Table 3
[0188]
[0189] It can be seen from the results in Table 3 that compared with DA1 to DA3, the A0 of the composite catalytic materials A1 to A12 prepared according to the method disclosed in the present invention is 10 to 20%, and the catalytic activity is high. The metal-containing multi-level porous heteroatom molecular sieve composite catalytic material is used for the low-temperature oxidation reaction of VOCs, which can obtain a higher VOCs conversion rate and complete combustion product selectivity.
[0190] Comparing the catalytic effects of A1 to A12, it can be seen that compared with A12, the A0 of A1 to A11 is between 10 and 18%, which can obtain higher VOCs conversion rate and complete combustion product selectivity.
[0191] Reaction Examples 2 to 4
[0192] To illustrate the effects of oxidation reactions of different VOCs gases and the effects under different oxidation reaction conditions, the specific reaction conditions and reaction results are listed in the following Table 4, where the catalyst addition amount is 0.5 g.
[0193] Table 4
[0194]
[0195] According to the data in Table 5, compared with Reaction Example 2, the GHSV of VOCs in Reaction Example 1 using the same catalyst A3 is 5000h -1 , the VOCs conversion rate and the complete combustion product selectivity in Example 1 are higher.
[0196] Comparing Reaction Example 3 with Reaction Example 4, the reaction temperature in Reaction Example 3 satisfies 150-250° C., and the VOCs conversion rate and complete combustion product selectivity in Reaction Example 3 are higher.
[0197] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0198] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0199] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A VOCs gas oxidation method, characterized in that: The following steps are involved: In the presence of oxygen, VOCs gas is brought into contact with a catalyst for oxidation reaction; the catalyst is a composite catalytic material, the composite catalytic material comprises a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve, the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, the heteroatom element Q is selected from one or more of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; The conditions of the oxidation reaction include: the volume ratio of oxygen to VOCs gas is 1-10:1, the gas volume space velocity of VOCs is 3000-6000h -1 , the reaction temperature is 150~300℃, and the reaction time is 1~48h; The composite catalytic material has the following UV-Vis characteristics: The peak area of the spectrum peak in the wavelength range of 460-540nm obtained by the peak separation result of the wavelength of 460-740nm in the UV-Vis spectrum of the composite catalyst material is recorded as A1, and the total peak area in the wavelength range of 460-740nm in the UV-Vis spectrum of the composite catalyst material is recorded as A2; A0 defined by the following formula (1) is any value between 10% and 20%; A0=A1 / A2 (1); The framework heteroatom molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve; In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1; The molar ratio of metal M element to silicon element is (0.001~0.2):1; The BET specific surface area of the composite catalytic material is 360-800 m 2 / g, the total pore volume is 0.30~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.18~0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~4.5nm.
2. The method according to claim 1, characterized in that The conditions of the oxidation reaction include: the volume ratio of oxygen to VOCs gas is 4-10:1; the gas volume space velocity of VOCs is 3000-5000 h -1 ; The reaction temperature is 150~250℃; The reaction time is 2~24h.
3. The method according to claim 1, characterized in that: The VOCs are one or more selected from non-methane hydrocarbons, oxygen-containing organic compounds, halogenated hydrocarbon compounds, nitrogen-containing organic compounds and sulfur-containing organic compounds.
4. The method according to claim 3, characterized in that The non-methane hydrocarbon is selected from one or more of ethane, ethylene, acetylene, benzene, xylene, styrene and naphthalene; The oxygen-containing organic compound is selected from one or more of methyl tert-butyl ether, formaldehyde, benzaldehyde and phenol; The halogenated hydrocarbon compound is selected from one or more of trichloroethylene, chloroform and trichloroethane; The nitrogen-containing organic compound is selected from one or more of diisocyanate compounds having 1 to 16 carbon atoms, diisocyanatolyl compounds having 1 to 16 carbon atoms, amine compounds having 1 to 16 carbon atoms, and amide compounds having 1 to 16 carbon atoms; The sulfur-containing organic compound is selected from one or more of sulfide compounds having 2 to 16 carbon atoms, thiol compounds having 1 to 16 carbon atoms, and thiophene compounds having 4 to 16 carbon atoms.
5. The method according to claim 4, characterized in that The nitrogen-containing organic compound is selected from one or more of aniline, propionamide and toluene diisocyanate; The sulfur-containing organic compound is selected from one or more of benzothiophene, methyl mercaptan and dimethyl sulfide.
6. The method according to claim 1, characterized in that The reactor for the oxidation reaction is selected from any one of a tank reactor, a fixed bed reactor, a moving bed reactor, a suspended bed reactor or a slurry bed reactor.
7. The method according to claim 1, characterized in that The A0 is any value between 10% and 18%.
8. The method according to claim 1, characterized in that The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
9. The method according to claim 8, characterized in that The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.
10. The method according to claim 1, characterized in that In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.043): 1; The molar ratio of metal M element to silicon element is (0.001~0.16):
1.
11. The method according to claim 1, characterized in that: The composite catalytic material is prepared by a preparation method comprising the following steps: S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments; The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.
12. The method according to claim 11, characterized in that In step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005~1): (0.001~0.05): (10~80): (0.002~0.2): (0.015~0.4); the molar ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01~3):
1.
13. The method according to claim 12, characterized in that In step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005~1): (0.002~0.043): (10~80): (0.001~0.165): (0.015~0.3); the molar ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01~2):
1.
14. The method according to claim 11, characterized in that Step S1 includes the following steps: a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution; b. adding the dendritic macromolecule to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.
15. The method according to claim 14, characterized in that The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
16. The method according to claim 11, characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
17. The method according to claim 16, characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
18. The method according to claim 17, characterized in that The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
19. The method according to claim 18, characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
20. The method according to claim 19, characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
21. The method according to claim 18, characterized in that The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
22. The method according to claim 11, characterized in that The template agent is an organic base.
23. The method according to claim 22, characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
24. The method according to claim 23, characterized in that The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): Formula (B); wherein R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms.
25. The method according to claim 24, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.
26. The method according to claim 25, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
27. The method according to claim 11, characterized in that The molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
28. The method according to claim 14, characterized in that In step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
29. The method according to claim 28, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
30. The method according to claim 11, characterized in that In step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one selected from chlorides, nitrates and sulfates of heteroatom element Q; the organic skeleton heteroatom precursor is an organic acid ester containing heteroatom element Q, selected from at least one of the structures shown in the following formula (C): Formula (C); wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms.
31. The method according to claim 30, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms.
32. The method according to claim 31, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 2 to 4 carbon atoms and a branched alkyl group having 2 to 4 carbon atoms.
33. The method according to claim 30, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl and isohexyl.
34. The method according to claim 33, characterized in that In formula (C), R5, R6, R7 and R8 are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
35. The method according to claim 1, characterized in that When the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is boron, the skeleton heteroatom precursor is selected from one or more of boric acid and borate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is aluminum, the skeleton heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; when the skeleton heteroatom is phosphorus, the skeleton heteroatom precursor is selected from one or more of orthophosphoric acid, triethyl phosphoric acid and metaphosphate; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.
36. The method according to claim 11, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M.
37. The method according to claim 36, characterized in that The metal M precursor is a water-soluble inorganic salt of the metal element M.
38. The method according to claim 37, characterized in that The metal M precursor is an aqueous solution of the metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1: (50-500).
39. The method according to claim 11, characterized in that In step S1, the dendritic macromolecules are selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules.
40. The method according to claim 39, characterized in that The polyamide-amine macromolecule is selected from one or more of the second generation PAMAM with an ethylenediamine core, the third generation PAMAM with an ethylenediamine core, and the fourth generation PAMAM with an ethylenediamine core; The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone.
41. The method according to claim 39, characterized in that The dendritic macromolecule has a weight average molecular weight of 4000-85000, a viscosity of 0.025-0.045 dL / g at 30° C., and a branching degree of 4000-18000.
42. The method according to claim 11, characterized in that In step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amino group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amino group is independently selected from any integer in the range of 1 to 18, and the number of carbon atoms of the aromatic group is any integer in the range of 6 to 18.
43. The method according to claim 42, characterized in that The silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
44. The method according to claim 43, characterized in that The silanization agent is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
45. The method according to claim 11, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
46. The method according to claim 45, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.