A metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application
By introducing metal precursors and silanization reagents during the synthesis process of molecular sieves, composite catalytic materials of metal nanoparticles and molecular sieves are prepared, which solves the problem of simultaneous preparation of metal nanoparticles and hierarchical pore molecular sieves in the existing technology, and significantly improves the catalytic activity. The ability to react with macromolecules.
Patent Information
- Application Number
- CN202111422417.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-11-26
AI Technical Summary
It is difficult to achieve high dispersion of metal nanoparticles and molecular sieves and the preparation of multi-level pore molecular sieves at the same time with existing technology, resulting in reduced catalytic activity and limited pore structure, making it impossible to effectively catalyze macromolecular reactants.
By introducing metal precursors, silanization reagents and structural fillers during the molecular sieve synthesis process, and performing hydrothermal crystallization and roasting treatments, a composite catalytic material of metal nanoparticles and molecular sieves is prepared to ensure that the metal nanoparticles are evenly dispersed in the multi-stage pore molecular sieve. in the pores to improve catalytic activity.
The high specific surface area and pore volume of the composite material of metal nanoparticles and molecular sieves was achieved, and the macromolecule reaction activity was improved. In particular, the catalytic activity and selectivity were significantly improved in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
Smart Images

Figure CN116174011B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a metal nanoparticle and molecular sieve composite catalytic material and the preparation and application thereof. Background Art
[0002] Molecular sieves are good carriers for metal catalysts due to their high specific surface area, high thermal stability and high mechanical stability. In addition, the regular micropores and mesoporous structures of molecular sieves can play a selective role in the reaction (screening the reactants, reaction intermediates and products), and can play a synergistic or continuous catalytic role with the catalytic effect of the metal active center.
[0003] However, for metal catalysts, metal particles with high surface energy and surface tension are prone to sintering through Ostwald ripening or migration-agglomeration processes in high temperature or hydrothermal environments, resulting in increased particle size and decreased catalytic activity. In theory, there are two main strategies to improve the sintering resistance of metal particles: (1) Enhance the interaction between nanoparticles and carriers. For example, metal nanoparticles are easily activated with some reducing oxide carriers (such as TiO2, CeO2, etc.) under certain conditions to form a strong metal-support interaction (SMSI). At this time, there is generally a significant electronic offset between the metal and the carrier, and the carrier may cover the surface of the metal particles by wrapping, modifying or migrating, which has a strong stabilizing and binding effect on the metal, significantly enhancing the sintering resistance of the metal. (2) Encapsulate metal nanoparticles in a medium with weak metal-support interaction such as oxides, mesoporous materials or molecular sieves, and use confinement to block the thermal migration path of metal particles.
[0004] Usually, it is difficult to highly disperse metals into molecular sieve crystals by conventional impregnation methods. This is because the micropores of molecular sieves are small in size, and the impregnation method usually uses metal salt solutions for impregnation. The size of metal hydrated ions is generally larger than the pore size of the molecular sieve and cannot diffuse into the pores. They can only gather on the outer surface of the molecular sieve particles. In response to this, researchers have developed two series of preparation methods: direct synthesis and post-synthesis.
[0005] The direct synthesis method generally refers to the direct introduction of metal precursors during the crystallization of molecular sieves. During the hydrothermal crystallization process, the metal precursors can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structural units, the metal nanoparticles are evenly embedded in the molecular sieve framework. Since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursors are very easy to form hydroxide precipitation. In order to solve this problem, the precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.). For example, Wang et al. used ethylenediamine ligands and PdCl2 to form [Pd(NH2CH2CH2NH2)]Cl2 complex precursors, and then directly synthesized silicalite-1 molecular sieves (Pd@silicalite-1) with uniformly dispersed Pd nanoparticles embedded by hydrothermal crystallization.
[0006] Due to the limitation of pores, microporous molecular sieves can only be diffused by reactants of small molecular size, and thus cannot catalyze reactions involving macromolecular substrates. To address this defect, mesopores and even macropores are introduced into microporous molecular sieves to construct molecular sieves with multi-level pore sizes, thereby improving the performance of microporous molecular sieves when applied to macromolecular reactants. According to different synthesis methods, the synthesis methods of multi-level pore molecular sieves mainly include the removal of skeleton atoms, the dual template synthesis method of ordered micro-mesoporous composite molecular sieves, the hard template method, the dry gel conversion method and the silanization method. Among them, the silanization method is relatively simple and widely used.
[0007] However, it is still difficult to simultaneously achieve the two goals of "complexing metal precursors with organic ligands and then introducing them into the hydrothermal crystallization process of the molecular sieve to highly disperse the nanoparticles in the molecular sieve crystals" and "preparing multi-level pore molecular sieves by silanization" to obtain molecular sieves with the advantages of both. In other words, it is impossible to directly prepare multi-level pore molecular sieves with highly dispersed metals. Summary of the invention
[0008] The purpose of the present disclosure is to provide a metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The composite material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal nanoparticles have uniform particle size and are evenly dispersed in the molecular sieve pores.
[0009] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, including an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal element M is a metal element that can form an oxide aggregate; the composite catalytic material has the following XPS characteristics: the electron binding energy of the metal element M in the composite catalytic material is denoted as T1, and the electron binding energy of the metal element M in the oxide aggregate is denoted as T2, and T0 defined by the following formula (1) is any value between 0.5 and 1.0 eV; T0 = T1-T2 formula (1).
[0010] Optionally, the value of T0 is any value between 0.55 and 0.85 eV.
[0011] Optionally, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0012] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0013] Optionally, the metal M is Co, and the oxide aggregate is a Co3O4 aggregate;
[0014] The metal M is Mn, and the oxide aggregate is a MnO2 aggregate;
[0015] The metal M is Fe, and the oxide aggregate is Fe2O3 aggregate;
[0016] The metal M is Ni, and the oxide aggregate is NiO aggregate;
[0017] The metal M is Pd, and the oxide aggregate is a PdO aggregate;
[0018] The metal M is Pt, and the oxide aggregate is a PtO2 aggregate; or
[0019] The metal M is Cu, and the oxide aggregate is CuO aggregate;
[0020] Preferably, when the metal element M is Co, Mn, Fe, Ni or Cu, the electron binding energy of the metal element M is 2p 3 / 2When the metal element M is Pt, the electron binding energy of the metal element M is 4f 7 / 2 When the metal element M is Pd, the electron binding energy of the metal element M is 3d 5 / 2 The binding energy of an electron.
[0021] Optionally, in the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.001-0.15):1.
[0022] Optionally, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.15-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-10nm.
[0023] A second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:
[0024] S1. Mixing a template, a silicon source, water, a metal M precursor, a silanization agent and a structural filler to obtain a reaction mixture, wherein the structural filler is an amphiphilic surfactant and / or a hard template; S2. Performing a hydrothermal crystallization treatment and a calcination treatment on the reaction mixture.
[0025] Optionally, in step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent is 1: (0.001-1): (5-100): (0.001-0.2): (0.025-0.4); preferably 1: (0.005-0.5): (5-100): (0.001-0.15): (0.025-0.3); the weight ratio of SiO2 to structural filler in the reaction mixture is (3-100): 1.
[0026] Optionally, step S1 includes:
[0027] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0028] b. mixing the metal M precursor and the hydrolyzed silicon solution to obtain a first mixed material;
[0029] c. Adding a silanization agent and a structural filler to the first mixed material respectively, and mixing them to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0030] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0031] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0032]
[0033] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0034] Optionally, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0035] R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from at least one of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group and a tert-butyl group;
[0036] Further preferably, the all-silicon molecular sieve is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or the all-silicon molecular sieve is an MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or the molecular sieve is a Beta type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0037] Optionally, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0038] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0039] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0040] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0041] Preferably, the metal M precursor is in the form of an aqueous solution of the metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0042] Optionally, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group, and the amine group are each independently 1 to 18, and the number of carbon atoms of the aromatic group is 6 to 18;
[0043] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0044] Optionally, in step S1, the structural filler is selected from one or more of cetyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, PEO-PPO-PEO triblock copolymer, mesoporous carbon and natural cellulose.
[0045] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 10 days, the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, the hydrothermal crystallization temperature is 150 to 200° C.; the pressure is autogenous pressure;
[0046] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0047] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0048] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0049] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and a preparation method and application thereof. The metal nanoparticle and molecular sieve composite material provided by the present disclosure is prepared by adding a metal precursor, a silanization agent and a macromolecular structure filler to a crystallization system at the same time. The molecular sieve of the composite material has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal nanoparticles have a uniform particle size and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; when the XPS binding energy of the metal M element in the composite material is 0.5 to 1.0 eV higher than the XPS binding energy of the metal M element in the oxide aggregate of the metal M, the composite material has a high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0050] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0052] Figure 1 This is the SEM spectrum of the product prepared in Example 1 of the present disclosure.
[0053] Figure 2 This is the XRD spectrum of the product prepared in Example 1 of the present disclosure.
[0054] Figure 3 This is the TEM spectrum of the product prepared in Example 1 of the present disclosure.
[0055] Figure 4 This is the infrared (FT-IR) spectrum of the product prepared in Example 1 of the present disclosure.
[0056] Figure 5 This is the ultraviolet-visible diffuse reflectance (UV-Vis) spectrum of the product prepared in Example 1 of the present disclosure.
[0057] Figure 6 This is the EDX spectrum of the product prepared in Example 1.
[0058] Figure 7 This is the XRD spectrum of the product prepared in Example 10.
[0059] Figure 8 This is the XRD spectrum of the product prepared in Example 11.
[0060] Fig. 9 This is the metal element Co XPS spectrum of the product prepared in Example 1. DETAILED DESCRIPTION
[0061] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0062] The inventors of the present disclosure surprisingly found in experiments that after introducing a metal precursor during the synthesis of the molecular sieve, and then continuously introducing a silanization agent and a structural filler, and subjecting the obtained mixture to hydrothermal crystallization, washing and calcination, the obtained composite catalytic material including all-silicon molecular sieve and metal M oxide nanoparticles not only has large specific surface area and pore volume performance, but also has uniform particle size of the metal oxide nanoparticles and is evenly dispersed in the pores of the molecular sieve. Moreover, when the value of T0 (i.e., T1-T2) in the composite material is above 0.5 eV (T1 represents the XPS binding energy of the metal M element in the composite catalytic material, and T2 represents the XPS binding energy of the metal M element in the oxide aggregates of the metal M), the composite material has good catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins. For example, when used in the co-oxidation reaction of cyclooctene and isobutyraldehyde, a higher cyclooctene conversion rate and epoxycyclooctene selectivity can be obtained.
[0063] The first aspect of the present disclosure provides a metal oxide nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal element M is a metal element capable of forming oxide aggregates;
[0064] The composite catalytic material has the following XPS characteristics:
[0065] The electron binding energy of the metal element M in the composite catalyst material is denoted as T1,
[0066] The electron binding energy of the metal element M in the oxide aggregate is denoted as T2, and T0 defined by the following formula (1) is any value between 0.5 and 1.0 eV;
[0067] T0=T1-T2 formula (1).
[0068] The present invention provides a composite catalytic material of metal oxide nanoparticles and molecular sieves. The molecular sieve of the composite material has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; when the XPS binding energy of the metal M element in the composite material is 0.5 to 1.0 eV higher than the XPS binding energy of the metal M element in the oxide aggregate of the metal M, the composite material has a high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0069] In the present disclosure, metal M oxide aggregates refer to conventional oxide types obtained by calcining metal M precursors (such as nitrates, chlorides, etc.) known in the art during the synthesis of molecular sieves, for example, the oxide aggregates of metal cobalt are Co3O4 and the oxide aggregates of metal Cu are CuO.
[0070] In a preferred embodiment, the value of T0 is any value between 0.55 and 0.85 eV. When T0 of the composite catalyst material is within this range, it has higher catalytic activity, cyclooctene conversion rate and epoxycyclooctene selectivity.
[0071] In one embodiment, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0072] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; preferably selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum and copper.
[0073] In an optional embodiment, the metal M is Co, and the oxide aggregate is a Co3O4 aggregate;
[0074] In an optional embodiment, the metal M is Mn, and the oxide aggregate is a MnO2 aggregate;
[0075] In an optional embodiment, the metal M is Fe, and the oxide aggregate is Fe2O3 aggregate;
[0076] In an optional embodiment, the metal M is Ni, and the oxide aggregate is NiO aggregate;
[0077] In an optional embodiment, the metal M is Pd, and the oxide aggregate is a PdO aggregate;
[0078] In an optional embodiment, the metal M is Pt, and the oxide aggregate is a PtO2 aggregate;
[0079] In an optional embodiment, the metal M is Cu, and the oxide aggregate is CuO aggregate;
[0080] Preferably, when the metal element M is Co, Mn, Fe, Ni or Cu, the electron binding energy of the metal element M is 2p 3 / 2 When the metal element M is Pt, the electron binding energy of the metal element M is 4f 7 / 2When the metal element M is Pd, the electron binding energy of the metal element M is 3d 5 / 2 The binding energy of an electron.
[0081] In one embodiment, in the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.001-0.15):1.
[0082] In one embodiment, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, the average particle size of the metal nanoparticles is 0.5 to 10 nm, preferably 0.5 to 5 nm; the BET specific surface area is 400 to 800 m 2 / g, preferably 400 to 700 m 2 / g; total pore volume is 0.3-0.65mL / g, preferably 0.31-0.63mL / g; micropore volume is 0.1-0.19mL / g, preferably 0.11-0.18mL / g; mesopore volume is 0.15-0.46mL / g, preferably 0.17-0.46mL / g. The composite catalytic material disclosed in the present invention also has a multi-level pore structure, which is conducive to catalyzing reaction substrates of different sizes, especially suitable for catalyzing macromolecular substrate reactions.
[0083] A second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:
[0084] S1, mixing a template, a silicon source, water, a metal M precursor, a silanization agent and a structural filler to obtain a reaction mixture, wherein the structural filler is an amphiphilic surfactant and / or a hard template;
[0085] S2. performing hydrothermal crystallization and calcination on the reaction mixture.
[0086] The present invention introduces metal precursors, silanization agents and macromolecular structure fillers into the molecular sieve synthesis raw materials, which can take into account the effects of highly dispersed metal oxide nanoparticles and molecular sieve support layer pore expansion, and prepare a multi-level porous molecular sieve composite catalytic material with highly dispersed metal oxide nanoparticles.
[0087] In the present disclosure, metal ions form a complex with a silanization agent, and the metal oxide nanoparticles in the molecular sieve pores obtained after hydrothermal crystallization and calcination have high dispersion; and the silanization agent silanol group and the organosilicon source silanol group hydrolyze and condense to produce a stable Si-O-Si bond, thereby ensuring the realization of the supporting layer pore expansion effect. In addition, the long carbon chain of the silanization agent and the structural filler of the amphiphilic surfactant can form a stable and controllable structural unit (the long carbon chain of the silanization agent and the hydrophobic group of the surfactant are close to each other and interact with each other by van der Waals force), thereby playing a fine adjustment role in the supporting layer pore expansion; or a hard template agent with controllable size is used to play a role in space filling. The molecular sieve of the composite catalytic material finally obtained produces an ordered, pore-controlled (controlled by the chain length of the silanization agent alkyl chain) mesoporous structure. And the metal M oxide nanoparticles formed by the metal M introduced in the molecular sieve synthesis process can also be uniformly dispersed in the mesoporous pores of the multi-level pore molecular sieve.
[0088] In one embodiment, in step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent is 1: (0.001-1): (5-100): (0.001-0.2): (0.025-0.4); preferably 1: (0.005-0.5): (5-100): (0.001-0.15): (0.025-0.3); the weight ratio of SiO2 to structural filler in the reaction mixture is (3-100): 1. Specifically, the water used in step S1 can be water commonly used in the synthesis of molecular sieves, and in order to avoid the introduction of heteroatoms, it is preferably deionized water.
[0089] In a preferred embodiment, step S1 comprises:
[0090] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0091] b. mixing the metal M precursor and the hydrolyzed silicon solution to obtain a first mixed material;
[0092] c. Adding a silanization agent and a structural filler to the first mixed material respectively, and mixing them to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0093] In one embodiment, in step S1, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black; the general formula of the organic silicone grease is the structure shown in the following formula (A):
[0094]
[0095] Where Ra , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight chain alkyl group having 1 to 4 carbon atoms or a branched chain alkyl group having 3 to 4 carbon atoms. a , R b , R c , R d Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl. a , R b , R c , R d Each is independently methyl or ethyl.
[0096] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0097] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.
[0098] Further preferably, the template is selected from at least one of the quaternary ammonium bases having the following general formula (B):
[0099] R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0100] The template agent is preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide (including various isomers of tetrapropylammonium hydroxide, such as tetra-n-propylammonium hydroxide and tetraisopropylammonium hydroxide) and tetrabutylammonium hydroxide (including various isomers of tetrabutylammonium hydroxide, such as tetra-n-butylammonium hydroxide and tetraisobutylammonium hydroxide).
[0101] In a preferred embodiment, the all-silicon molecular sieve is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or in another preferred embodiment, the all-silicon molecular sieve is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or, in another preferred embodiment, the molecular sieve is a Beta type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide. The present disclosure can prepare molecular sieves of different structures by selecting different template agents.
[0102] In one embodiment, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0103] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95°C for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95°C for 2 to 8 hours;
[0104] Preferably, the hydrolysis-alcohol removal treatment is performed so that the mass content of alcohol produced by hydrolysis of the obtained organic silicone grease in the hydrolysis solution of silicon is less than 10 ppm.
[0105] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal (such as a compound containing a metal element and / or a metal single substance) can achieve the purpose of the present disclosure.
[0106] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the organic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0107] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0108] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0109] In one embodiment, in step S1, the general formula of the silanization reagent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group, and the amine group are each independently 1 to 18, preferably 1 to 12; the number of carbon atoms of the aromatic group can be 6 to 18, preferably 6 to 12.
[0110] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0111] In one embodiment, in step S1, the structural filler is selected from one or more of cetyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, PEO-PPO-PEO triblock copolymer, mesoporous carbon and natural cellulose.
[0112] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; the pressure is autogenous pressure.
[0113] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.
[0114] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0115] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0116] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite material is 1 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.
[0117] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.
[0118] The present disclosure will be further described below using examples.
[0119] In the present disclosure, the X-ray diffraction (XRD) crystal phase diagram of the sample is measured on a Siemens D5005 X-ray diffractometer, the radiation source is Kα (Cu), and the test range 2θ is 0.5° to 70°.
[0120] The Fourier transform infrared (FT-IR) spectra of the samples were measured on a Nicolet 8210 Fourier transform infrared spectrometer in the range of 400 to 4000 cm -1 .
[0121] The UV-visible diffuse reflectance spectrum (UV-vis) of the samples was measured on a SHIMADZU UV-3100 UV-visible spectrometer in the range of 400 to 4000 cm -1 .
[0122] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.
[0123] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.
[0124] The XPS characterization of the samples was carried out on an ESCALAB 250 X-ray photoelectron spectrometer with monochromatic Al Kα X-rays, energy of 1486.6 eV, power of 150 W, and the C1s peak (284.8 eV) of contaminated carbon was used to correct the nuclear charge shift.
[0125] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0126] The cobalt nitrate used in the embodiments of the present disclosure is cobalt nitrate hexahydrate.
[0127] Example 1
[0128] (1) 1.6 g of a 25.05 wt% tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol, SiO2 mass 6 g) and 52.8 g of water (3 mol) were added to a 500 mL beaker in sequence, placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;
[0129] (2) 0.03 g of cobalt nitrate hexahydrate (0.0001 mol) and 0.18 g (0.01 mol) of water were stirred to obtain a cobalt aqueous solution, and the cobalt aqueous solution was mixed with the hydrolyzed silicon solution obtained in step (1);
[0130] (3) adding 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) and 0.3 g of PEO-PPO-PEO triblock copolymer (P123, purchased from Inotech, weight average molecular weight 5800) to the mixture of step (2), and stirring for 0.5 hour;
[0131] (4) The mixture obtained in step (3) is transferred to a stainless steel closed reactor and crystallized at a constant temperature of 175° C. for 24 hours to obtain a sample. The obtained sample is filtered, washed, dried at 110° C. for 6 hours, and then calcined at 600° C. in a muffle furnace for 6 hours to obtain the metal oxide nanoparticle and molecular sieve composite material product of the present invention, which is recorded as CAT-1.
[0132] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of the metal nanoparticles contained in the composite catalytic material of CAT-1 are listed in Table 2.
[0133] The SEM image of CAT-1 is as follows: Figure 1 The XRD spectrum of CAT-1 is shown in Figure 2 As shown in Figure 2, XRD analysis shows that it has an MFI structure; the TEM image of CAT-1 is shown in Figure 2. Figure 3 As shown; the infrared spectrum of CAT-1 is as shown Figure 4The UV-visible spectrum of CAT-1 is shown in the figure. Figure 1 , Figure 3 It can be seen that the product CAT-1 prepared in this example has a regular shape and uniform size; Figure 4 Medium 960cm -1 The characteristic peaks nearby indicate that Co is bound to the surface of the silicon skeleton; Figure 5 The characteristic peaks at 450-700 nm indicate that there is interaction between Co and Si. The EDX images obtained from the TEM test of CAT-1 are shown in Figure 6 As shown, it can be seen that the metal Co is evenly dispersed in the molecular sieve. The XPS spectrum of the metal element Co of CAT-1 is shown in Fig. 9 shown.
[0134] Comparative Example 1
[0135] This comparative example was prepared according to the method of Example 1, except that no silanization agent and structural filler were added. The ratio, synthesis conditions and results are listed in Table 1. Other conditions and operations were similar to those of Example 1. The prepared product was recorded as Sample D-1.
[0136] Comparative Example 2
[0137] This comparative example was prepared according to the method disclosed in patent CN109821568 A.
[0138] 0.51g of cobalt nitrate hexahydrate, 1.28g of hexadecyltrimethylammonium bromide and 2.11g of sodium hydroxide were added to a flask, and then 65ml of deionized water was added, and the mixture was heated in a water bath at 40°C and stirred at 400 rpm for 2 hours. Ethyl orthosilicate was added dropwise to the above solution at a rate of 4 seconds / drop, and the final molar ratio of metal cobalt to silicon source was 0.08, and the mixture was stirred at 400 rpm for 24 hours. The silicate hydrate sol containing metal nitrate was transferred to a reactor, and the volume of the silicate hydrate sol accounted for about 70% of the reactor. The silicate hydrate sol was placed in a reactor for hydrothermal crystallization at 120°C for 24 hours. The product obtained in the above reactor was added to 30 times of its volume of deionized water, washed 3 times and centrifuged to neutrality, and the obtained product was dried at 100°C for 12 hours. The product was obtained by heating to 550°C at a rate of 1 degree / min and then calcining at 550°C for 300 min, and was recorded as D-2.
[0139] Comparative Example 3
[0140] This comparative example was prepared according to the method of Ning Wang et al. (JACS, 2016, Vol. 138, pp. 7484-7487).
[0141] First, deionized water was mixed with 13g TPAOH solution and stirred continuously for 10 minutes, and then 8.32g ethyl orthosilicate (0.04mol) was added. After continuous stirring for 6 hours, the mixture became clear after complete hydrolysis. 0.052g cobalt nitrate hexahydrate (0.18mmol, the molar ratio of metal cobalt to silicon source was 0.0045) was dissolved in a mixture of 0.3mL of ethylenediamine and 3mL of water to prepare [Pd(NH2CH2CH2NH2)2]Cl2 solution, and then the resulting solution was added dropwise to the above mixture and stirred for 30min without precipitation. The reaction mixture was transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner and static crystallization was performed at 170°C in a conventional oven for 4 days. The solid product was centrifuged, washed with water and ethanol several times, dried in an oven at 80°C overnight, roasted in an air atmosphere at 550°C for 8 hours, and finally reduced with hydrogen to obtain the product, which was recorded as D-3.
[0142] Embodiment 2 to Embodiment 9
[0143] The corresponding products CAT-2 to CAT-9 were prepared according to the method of Example 1. The proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1. SEM images of CAT-2 to CAT-9 and Figure 1 Similar XRD spectra and Figure 2 Similarly, XRD analysis shows that it has an MFI structure; TEM images are similar to Figure 3 Similar; FT-IR spectrum and Figure 4 Similar; UV-Vis spectra and Figure 5 resemblance.
[0144] Example 10
[0145] The cobalt-containing multi-level porous β molecular sieve was prepared by referring to the method of Example 1, and the ratio and template agent were changed. The template agent used was tetraethylammonium hydroxide (TEAOH). The ratio and synthesis conditions and results are shown in Table 1. The obtained product was recorded as CAT-10. The XRD spectrum of the obtained product is shown in Figure 7 As shown, it has a β molecular sieve structure.
[0146] Embodiment 11
[0147] The cobalt-containing multi-level porous MEL molecular sieve was prepared in practice. The ratio and template agent were changed by referring to the method of Example 1. The template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product was recorded as CAT-11. The XRD spectrum of the obtained product is shown in Figure 8 As shown, it has a MEL molecular sieve structure.
[0148] Example 12
[0149] The cobalt-containing multi-level porous MFI molecular sieve was prepared by referring to the method of Example 1, and the proportions, synthesis conditions and results are shown in Table 1. The obtained product is recorded as CAT-12. The hydrothermal crystallization temperature is 140°C and the hydrothermal crystallization time is 7 days; the calcination temperature is 840°C and the calcination time is 9 hours.
[0150] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of metal nanoparticles contained in the composite materials of the products obtained in the above examples and comparative examples are listed in Table 2 below.
[0151] Table 1
[0152]
[0153]
[0154] In Table 1, TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane); P123 is PEO-PPO-PEO triblock copolymer, CTAB is hexadecyltrimethylammonium bromide, and SDBS is sodium dodecylbenzene sulfonate. The reagents used in the present disclosure can be obtained through conventional purchasing channels.
[0155] Table 2
[0156]
[0157] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0158] According to Table 2, compared with D-1 prepared in Comparative Example 1 (without adding silanizing agent and structural filler) and D-3 prepared in Comparative Example 3 (without adding silanizing agent and structural filler), silanizing agent and structural filler are added during the preparation process of Examples 1 to 12 of the present disclosure, and the obtained products CAT-1 to CAT-12 have higher mesopore volumes, indicating that the method provided in the present disclosure can effectively expand the pores of the molecular sieve.
[0159] Test Case
[0160] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0161] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.
[0162] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):
[0163]
[0164]
[0165]
[0166] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1MPa, the amount of cyclooctene was 1mmol, the amount of catalyst was 50mg, and the amount of solvent acetonitrile was 2.5mL. The reaction was stable at 25°C for 6 hours, and the samples were taken for analysis. The results are shown in Table 3.
[0167] Table 3
[0168]
[0169] Among them, the T2 value of cobalt oxide aggregate Co3O4 is 781.25eV, the T2 value of nickel oxide aggregate NiO is 854.80eV, the T2 value of manganese oxide aggregate MnO2 is 642.10eV, the T2 value of copper oxide aggregate CuO is 933.60eV, and the T2 value of iron oxide aggregate Fe2O3 is 710.80eV.
[0170] According to the data in Table 3, compared with D-1 to D-3 prepared in comparative examples, the T0 of the metal oxide nanoparticles and molecular sieve composite catalytic materials CAT-1 to CAT-12 prepared in the embodiments of the present disclosure is between 0.5 and 1.0 eV, which has higher catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde, and higher cyclooctene conversion rate and epoxycyclooctene selectivity.
[0171] Comparing CAT-1 to CAT-11 with CAT-12, it can be seen that the T0 values of CAT-1 to CAT-11 are between 0.55 and 0.85 eV, and CAT-1 to CAT-11 have higher cyclooctene conversion rates, isobutyraldehyde conversion rates, and epoxycyclooctene selectivities.
[0172] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0173] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0174] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A composite catalytic material of metal nanoparticles and molecular sieves, It is characterized in that It comprises an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal element M is a metal element capable of forming oxide aggregates; the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; The composite catalytic material has the following XPS characteristics: The electron binding energy of the metal element M in the composite catalyst material is denoted as T 1 , The electron binding energy of the metal element M in the oxide aggregate is denoted as T 2 , T is defined as follows: 0 Any value between 0.5 and 1.0 eV; T 0 = T 1 -T 2 Formula (1); The metal nanoparticle and molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a silanization agent and a structural filler to obtain a reaction mixture, wherein the structural filler is an amphiphilic surfactant and / or a hard template; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatment; Wherein, the general formula of the silanization agent is R 5 Si(R 6 )(R 7 )R 8 , where R 5 , R 6 , R 7 , R 8 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R 5 , R 6 , R 7 , R 8 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amine group is independently any integer from 1 to 18, and the number of carbon atoms of the aromatic group is any integer from 6 to 18.
2. The composite catalytic material according to claim 1, It is characterized in that The T 0 The value is any value between 0.55 and 0.85 eV.
3. The composite catalytic material according to claim 1, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.
4. The composite catalytic material according to claim 3, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the group consisting of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
5. The composite catalytic material according to claim 4, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, the MEL structure molecular sieve and the BEA structure molecular sieve.
6. The composite catalytic material according to claim 1, It is characterized in that The metal M is Co, and the oxide aggregate is Co 3 O 4 Aggregates; The metal M is Mn, and the oxide aggregate is MnO 2 Aggregates; The metal M is Fe, and the oxide aggregate is Fe 2 O 3 Aggregates; The metal M is Ni, and the oxide aggregate is NiO aggregate; The metal M is Pd, and the oxide aggregate is a PdO aggregate; The metal M is Pt, and the oxide aggregate is PtO 2 Aggregates; or The metal M is Cu, and the oxide aggregate is CuO aggregate.
7. The composite catalytic material according to claim 6, It is characterized in that When the metal element M is Co, Mn, Fe, Ni or Cu, the electron binding energy of the metal element M is 2p 3 / 2 When the metal element M is Pt, the electron binding energy of the metal element M is 4f 7 / 2 When the metal element M is Pd, the electron binding energy of the metal element M is 3d 5 / 2 The binding energy of an electron.
8. The composite catalytic material according to claim 1, It is characterized in that In the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.2):
1.
9. The composite catalytic material according to claim 8, It is characterized in that In the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.15):
1.
10. The composite catalytic material according to claim 1, It is characterized in that The BET specific surface area of the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, and the mesopore volume is 0.15~0.46mL / g; The metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-10 nm.
11. The composite catalytic material according to claim 1, It is characterized in that In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent is 1: (0.001-1): (5-100): (0.001-0.2): (0.025-0.4).
12. The composite catalytic material according to claim 11, It is characterized in that In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent is 1: (0.005-0.5): (5-100): (0.001-0.15): (0.025-0.3); SiO in the reaction mixture 2 The weight ratio to structural filler is (3~100):
1.
13. The composite catalytic material according to claim 1, It is characterized in that Step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. mixing the metal M precursor and the hydrolyzed silicon solution to obtain a first mixed material; c. Adding a silanization agent and a structural filler into the first mixed material respectively, and mixing them to obtain the reaction mixture.
14. The composite catalytic material according to claim 13, It is characterized in that The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
15. The composite catalytic material according to claim 1, It is characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
16. The composite catalytic material according to claim 15, It is characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
17. The composite catalytic material according to claim 16, It is characterized in that The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
18. The composite catalytic material according to claim 17, It is characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
19. The composite catalytic material according to claim 18, It is characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
20. The composite catalytic material according to claim 17, It is characterized in that The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
21. The composite catalytic material according to claim 1, It is characterized in that In step S1, the template agent is an organic base.
22. The composite catalytic material according to claim 21, It is characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
23. The composite catalytic material according to claim 22, It is characterized in that The template is selected from at least one of the quaternary ammonium bases having the following general formula (B): (B); R 1 , R 2 , R 3 and R 4 are independently selected from alkyl groups having 1 to 4 carbon atoms.
24. The composite catalytic material according to claim 23, It is characterized in that In formula (B), R 1 , R 2 , R 3 and R 4 are independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms.
25. The composite catalytic material according to claim 24, It is characterized in that In formula (B), R 1 , R 2 , R 3 and R 4 Each of the at least one groups is selected from the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
26. The composite catalytic material according to claim 1, It is characterized in that The all-silicon molecular sieve is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or the all-silicon molecular sieve is an MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or the molecular sieve is a Beta type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
27. The composite catalytic material according to claim 13, It is characterized in that In step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain a hydrolyzed solution of the silicon; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
28. The composite catalytic material according to claim 27, It is characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
29. The composite catalytic material according to claim 1, It is characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M.
30. The composite catalytic material according to claim 29, It is characterized in that The metal M precursor is a water-soluble inorganic salt of metal M.
31. The composite catalytic material according to claim 30, It is characterized in that The metal M precursor is in the form of an aqueous solution of the metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
32. The composite catalytic material according to claim 1, It is characterized in that In step S1, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
33. The composite catalytic material according to claim 32, It is characterized in that The silanization agent is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
34. The composite catalytic material according to claim 1, It is characterized in that In step S1, the structural filler is selected from one or more of cetyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, PEO-PPO-PEO triblock copolymer, mesoporous carbon and natural cellulose.
35. The composite catalytic material according to claim 1, It is characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
36. The composite catalytic material according to claim 35, It is characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.
37. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 36 in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins.