Catalytic material comprising molecular sieve and metal element and preparation method and application thereof

By introducing metal precursors, dendrimers and silanization reagents during the synthesis process of molecular sieves, composite catalytic materials of metal nanoparticles and molecular sieves are prepared, which solves the problems of dispersion and hierarchical pore structure of metal nanoparticles in molecular sieves and achieves High catalytic activity and improvement of macromolecular reactivity.

CN116174014BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111424576.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-15
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve high dispersion and hierarchical pore structure of metal nanoparticles in molecular sieves, while also solving the problem that metal precursors easily form hydroxide precipitation under high-temperature hydrothermal conditions.

Method used

By introducing metal precursors, dendrimers and silanization reagents during the synthesis process of molecular sieves, and performing hydrothermal crystallization and roasting treatments, composite catalytic materials of metal nanoparticles and molecular sieves are prepared, using the complexation and dendrimers of dendrimers. The supporting layer of the silanization reagent achieves a high degree of dispersion of metal nanoparticles and a hierarchical pore structure of the molecular sieve.

Benefits of technology

A composite catalytic material of metal nanoparticles and molecular sieves with large specific surface area, pore volume and high catalytic activity was obtained. The metal nanoparticles are uniform and evenly dispersed in the mesoporous channels of the molecular sieve, which significantly improves the activity of reacting with macromolecular substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174014B_ABST
    Figure CN116174014B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a catalytic material including a molecular sieve and a metal element, and a preparation method and application thereof. The composite catalytic material includes an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the composite catalytic material has the following IR-OH characteristics: the wave number in the IR-OH spectrum of the composite catalytic material is 3730-3740cm ‑1 The peak intensity of the highest peak in the range is recorded as I1; the wave number in the IR-OH spectrum of the all-silicon molecular sieve without the metal element M is 3730-3740cm ‑1 The peak intensity of the highest peak in the range is recorded as I2, and I0 defined by the following formula (1) is any value between 0.30 and 0.98; I0 = I1 / I2 formula (1). The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have uniform particle size and have a high dispersion in the molecular sieve crystal and on the pore surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a catalytic material comprising a molecular sieve and a metal element, and a preparation method and application thereof. Background Art

[0002] When introducing metal into molecular sieve, due to the small size of the micropores of molecular sieve, and the impregnation method usually uses metal salt solution for impregnation, the size of metal hydrated ions is generally larger than the pore size of molecular sieve, and cannot diffuse into the pores, and can only gather on the outer surface of molecular sieve particles. Therefore, it is usually difficult to use conventional impregnation methods to highly disperse metal nanoparticles into molecular sieve crystals. In order to disperse metal nanoparticles in molecular sieve crystals, researchers have developed two series of preparation methods: direct synthesis method and post-synthesis method.

[0003] The direct synthesis method generally refers to the direct introduction of metal precursors during the crystallization process of the molecular sieve. During the hydrothermal crystallization process, the metal precursor can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structure units, the metal nanoparticles are evenly embedded in the molecular sieve framework.

[0004] Due to the limitation of pores, microporous molecular sieves can only be diffused through by reactants of small molecular size, and thus cannot catalyze reactions involving macromolecular substrates. In view of this defect, mesopores or even macropores are introduced into microporous molecular sieves to construct molecular sieves with multi-level pore sizes, thereby improving the performance of microporous molecular sieves when applied to macromolecular reactants. According to different synthesis methods, the synthesis methods of multi-level pore molecular sieves mainly include the removal of skeleton atoms, the double template synthesis method of ordered micro-mesoporous composite molecular sieves, the hard template method, the dry gel conversion method and the silanization method. Among them, the silanization method is a relatively simple and widely used method. Since the silanol of the silanization agent hydrolyzes and condenses with the silanol of the molecular sieve precursor to produce a stable Si-O-Si bond, the effect of supporting layer pore expansion is ensured.

[0005] Wang Baorong et al. (CN 111847471 A) prepared a multi-level porous molecular sieve encapsulating active metals by introducing a silanization agent in a direct hydrothermal synthesis method. However, since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursor is very easy to form hydroxide precipitation. To solve this problem, the precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.), such as Wang et al. using ethylenediamine ligands and PdCl2 to form [Pd(NH2CH2CH2NH2)]Cl2 complex precursors, and then directly synthesized silicalite-1 molecular sieves (Pd@silicalite-1) with uniformly dispersed Pd nanoparticles embedded by hydrothermal crystallization.

[0006] Dendrimers are a new type of highly branched, symmetrical, radial functional polymers, also known as dendritic grafted macromolecules or ultra-high branched polymers. Due to their highly branched structure and unique monodispersity, these compounds have special properties and functions, and are widely used in research fields such as host-guest chemistry, catalysts, metal nanomaterials, nanocomposite catalytic materials, membrane materials, surfactants, and medicine. Their rich coordination sites, large-volume steric hindrance, and controllability are expected to be used in the synthesis of metal nanocatalysts.

[0007] In summary, the metal precursor is complexed with an organic ligand and then introduced into the hydrothermal crystallization process of the molecular sieve, which is a relatively effective method for highly dispersing nanoparticles in the molecular sieve crystal; and the silanization method of introducing a silanization agent into the molecular sieve synthesis process and expanding the pores by using the supporting effect of the alkyl chain is an effective and simple method for preparing multi-level pore molecular sieves. However, it is difficult to achieve the above two goals at the same time in general research, and obtain a molecular sieve with the advantages of both, that is, directly preparing a multi-level pore molecular sieve with highly dispersed metals. Summary of the invention

[0008] The purpose of the present disclosure is to provide a catalytic material including a molecular sieve and a metal element, and a preparation method and application thereof. The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have a uniform particle size and have a high dispersion in the molecular sieve crystal and on the pore surface.

[0009] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the composite catalytic material has the following IR-OH characteristics:

[0010] The wave number in the IR-OH spectrum of the composite catalyst material is 3730-3740 cm -1 The peak intensity of the highest peak in the range is recorded as I1; the wave number in the IR-OH spectrum of pure all-silicon molecular sieve is 3730-3740cm -1 The peak intensity of the highest peak in the range is recorded as I2.

[0011] I0 defined by the following formula (1) is any value between 0.30 and 0.98;

[0012] I0=I1 / I2 formula (1).

[0013] Optionally, the value of I0 is any value between 0.35 and 0.98.

[0014] Optionally, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;

[0015] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.

[0016] Optionally, in the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.2):1, preferably (0.001-0.16):1.

[0017] Optionally, the BET specific surface area of ​​the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.2-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-6nm.

[0018] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nano-oxide particles and molecular sieves, comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a dendritic macromolecule and a silanization agent to obtain a reaction mixture; S2, performing a hydrothermal crystallization treatment and a calcination treatment on the reaction mixture.

[0019] Optionally, in step S1, the molar ratio of silicon source calculated as SiO2: template: water: metal M element: silanization agent is 1: (0.005-1): (10-80): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-1): (10-80): (0.001-0.16): (0.025-0.3); the ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01-3): 1.

[0020] Optionally, step S1 includes:

[0021] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;

[0022] b. adding dendritic macromolecules to the aqueous solution of the metal M precursor, and mixing them to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;

[0023] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.

[0024] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably selected from at least one of organic silicone grease, solid silica gel and white carbon black; further preferably organic silicone grease, the general formula of the organic silicone grease is the structure shown in the following formula (A):

[0025]

[0026] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

[0027] Optionally, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):

[0028] R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from one of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group and a tert-butyl group;

[0029] Further preferably, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or

[0030] The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or

[0031] The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

[0032] Optionally, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;

[0033] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.

[0034] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;

[0035] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;

[0036] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).

[0037] Optionally, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms;

[0038] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0039] Optionally, in step S1, the dendritic macromolecule is selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules;

[0040] Preferably, the polyamidoamine macromolecule is selected from one or more of the 2nd generation PAMAM with an ethylenediamine core, the 3rd generation PAMAM with an ethylenediamine core, and the 4th generation PAMAM with an ethylenediamine core;

[0041] The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone;

[0042] Preferably, the dendrimer has a weight average molecular weight of 4000 to 85000, an intrinsic viscosity at 30° C. of 0.025 to 0.045 dL / g, and a degree of branching of 4000 to 18000 (in terms of Mw).

[0043] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;

[0044] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.

[0045] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.

[0046] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0047] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and a preparation method and application thereof. The present disclosure adds a metal precursor, a dendritic macromolecule and a silanization agent to the reaction raw materials synthesized by molecular sieve crystallization, so that the molecular sieve of the composite catalytic material prepared has a large specific surface area, pore volume and macromolecular substrate reaction activity; the molecular sieve of the composite catalytic material has a multi-level pore structure, and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the composite catalytic material has high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0048] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0050] Figure 1 This is the IR-OH spectrum of the product prepared in Example 1.

[0051] Figure 2 This is the XRD spectrum of the product prepared in Example 1.

[0052] Figure 3 This is the SEM image of the product prepared in Example 1. DETAILED DESCRIPTION

[0053] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0054] The first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve;

[0055] The composite catalytic material has the following IR-OH characteristics:

[0056] The wave number in the IR-OH spectrum of the composite catalyst material is 3730-3740 cm -1 The peak intensity of the highest peak in the range is recorded as I1; the wave number in the IR-OH spectrum of pure all-silicon molecular sieve is 3730-3740cm -1 The peak intensity of the highest peak in the range is recorded as I2.

[0057] I0 defined by the following formula (1) is any value between 0.30 and 0.98;

[0058] I0=I1 / I2 formula (1).

[0059] The molecular sieve of the composite catalytic material provided by the present invention has a large specific surface area, pore volume and reaction activity of macromolecular substrates; and the molecular sieve of the composite catalytic material has a multi-level pore structure, and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the composite catalytic material has high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0060] In the present disclosure, “pure all-silicon molecular sieve” refers to an all-silicon molecular sieve that does not contain other metal elements.

[0061] The wave number in the IR-OH spectrum of the composite catalytic material and the pure all-silicon molecular sieve described in the present disclosure is 3730-3740 cm -1 The peak intensity of the highest peak in the range may be a value obtained after the same normalization calculation. The normalization method is a method conventionally used in the art.

[0062] The inventors of the present disclosure surprisingly found in a large number of experimental studies that when a metal precursor, a dendritic macromolecule and a silanization agent are introduced into the molecular sieve synthesis process, after the reaction mixture is subjected to hydrothermal crystallization, washing and calcination, the obtained composite catalytic material including all-silicon molecular sieve and metal M oxide nanoparticles not only has a large specific surface area and pore volume performance, but also the metal oxide nanoparticles have uniform particle size and are evenly dispersed in the molecular sieve crystal (for example, in the molecular sieve mesopores), and may also exist on the surface of the molecular sieve pores; in addition, the inventors further found that the obtained composite catalytic material has a specific surface area of ​​3730-3740cm in the infrared hydroxyl (IR-OH) spectrum test. -1 The highest peak intensity (I1) in the range is 3730-3740 cm-1 in the IR-OH spectrum of the all-silicon molecular sieve without the metal element M. -1 The peak intensity (I2) of the highest peak in the range is low, that is, the terminal hydroxyl intensity is lower; and the ratio between I1 and I2 is related to the catalytic performance of the composite catalytic material, especially when I0 (I0=I1 / I2) is in the range of 0.30 to 0.98, the composite catalytic material has good catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins, for example, when used for the co-oxidation reaction of cyclooctene and isobutyraldehyde, a higher cyclooctene conversion rate and epoxycyclooctene selectivity can be obtained.

[0063] In the present disclosure, the infrared hydroxyl spectrum test of the composite catalytic material adopts the solid infrared hydroxyl spectrum test method, which is operated on NICOLET 6700. The following operations are included: (1) pressing about 20 mg of sample into a self-supporting sheet; (2) placing the sample sheet into a reaction cell and placing it under high vacuum of 1.0×10 -3Pa, and purify at 550°C for 2 hours; (3) the temperature is reduced to 150°C to measure the infrared spectrum.

[0064] In a preferred embodiment, the value of I0 is any value between 0.35 and 0.98. When the I0 of the composite catalytic material is within this range, a higher cyclooctene conversion rate and epoxycyclooctene selectivity can be achieved.

[0065] In one embodiment, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.

[0066] In one embodiment, the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.

[0067] In one embodiment, the composite catalytic material includes silicon element, metal element M and oxygen element, and the molar ratio of the metal element M to the silicon element is (0.001-0.2):1, preferably (0.001-0.16):1.

[0068] In one embodiment, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, the average particle size of the metal nanoparticles is 0.5 to 6 nm, preferably 0.5 to 4.5 nm, and the BET specific surface area is 400 to 800 m 2 / g, preferably 410 to 780 m 2 / g, the total pore volume is 0.3-0.65 mL / g, preferably 0.32-0.62 mL / g, the micropore volume is 0.1-0.19 mL / g, preferably 0.1-0.18 mL / g, and the mesopore volume is 0.2-0.46 mL / g, preferably 0.2-0.44 mL / g. The composite catalytic material disclosed in the present invention also has a multi-level pore structure, which is conducive to catalyzing reaction substrates of large molecular size.

[0069] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:

[0070] S1, mixing a template, a silicon source, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture;

[0071] S2. performing hydrothermal crystallization and calcination on the reaction mixture.

[0072] The present invention introduces metal precursors, dendritic macromolecules and silanization agents into the raw materials for molecular sieve crystallization synthesis, which can simultaneously achieve the effects of highly dispersing metal oxide nanoparticles in the molecular sieve crystals and expanding the pores of the molecular sieve support layer, thereby preparing a multi-level porous molecular sieve composite catalytic material with highly dispersed metal oxide nanoparticles.

[0073] In the present disclosure, on the one hand, the metal ions in the reaction mixture are complexed with the amino groups and other groups contained in the dendritic macromolecules to achieve the effect of dispersing and stabilizing the metal; at the same time, at least one coordination group (such as amino group, thiol group, oxygen-containing coordination group, etc.) carried by the silanization agent can also be complexed with the metal ions to achieve the effect of fixing and dispersing the metal, so that the metal oxide nanoparticles in the molecular sieve channels obtained after hydrothermal crystallization and calcination have high dispersion; on the other hand, the alkyl chain of the silanization agent also ensures the realization of the molecular sieve support layer expansion effect of the synthesized composite catalyst material, and the molecular volume of the dendritic macromolecule is very large, which can play a good role in supporting layer isolation during the crystallization of the molecular sieve. Thus, a multi-level porous all-silicon molecular sieve composite catalyst material with highly dispersed metal nanoparticles is finally prepared.

[0074] In the present disclosure, the "pure all-silicon molecular sieve" is a product obtained by using the same preparation method as the composite catalytic material (the same amount of reaction raw materials and reaction conditions, etc.) but without introducing the metal M precursor and dendritic macromolecules during the reaction process.

[0075] In one embodiment, in step S1, the molar ratio of silicon source calculated as SiO2: template: water: metal M element: silanization agent is 1: (0.005-1): (10-80): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-1): (10-80): (0.001-0.16): (0.025-0.3); the ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01-3): 1. Specifically, the water used in step S1 can be water commonly used in the synthesis of molecular sieves, and in order to avoid the introduction of heteroatoms, it is preferably deionized water.

[0076] In a preferred embodiment, step S1 comprises:

[0077] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;

[0078] b. adding dendritic macromolecules to the aqueous solution of the metal M precursor, and mixing them to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;

[0079] c. Adding a silanization agent to the second mixture, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.

[0080] In one embodiment, in step S1, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black; the general formula of the organic silicone grease is the structure shown in the following formula (A):

[0081]

[0082] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight chain alkyl group having 1 to 4 carbon atoms or a branched chain alkyl group having 3 to 4 carbon atoms. a , R b , R c , R d Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl. a , R b , R c , R d Each is independently methyl or ethyl.

[0083] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

[0084] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.

[0085] Further preferably, the template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B):

[0086] R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

[0087] The template agent is preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide (including various isomers of tetrapropylammonium hydroxide, such as tetra-n-propylammonium hydroxide and tetraisopropylammonium hydroxide) and tetrabutylammonium hydroxide (including various isomers of tetrabutylammonium hydroxide, such as tetra-n-butylammonium hydroxide and tetraisobutylammonium hydroxide).

[0088] In a preferred embodiment, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or

[0089] In another preferred embodiment, the molecular sieve of the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or

[0090] In another preferred embodiment, the molecular sieve of the composite catalyst material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide. The present disclosure can prepare molecular sieves of different structures by selecting different template agents.

[0091] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;

[0092] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.

[0093] Preferably, the hydrolysis-alcohol removal treatment is performed so that the mass content of alcohol produced by hydrolysis of the obtained organic silicone grease in the hydrolysis solution of silicon is less than 10 ppm.

[0094] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal (such as a compound containing a metal element and / or a metal single substance) can achieve the purpose of the present disclosure.

[0095] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the organic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;

[0096] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;

[0097] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).

[0098] In one embodiment, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, preferably 1 to 12 carbon atoms, and the aromatic group has 6 to 18 carbon atoms, preferably 6 to 12 carbon atoms;

[0099] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0100] In one embodiment, in step S1, the dendritic macromolecule is selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules.

[0101] In a preferred embodiment, the polyamide-amine macromolecule is selected from one or more of the 2nd generation PAMAM with an ethylenediamine core, the 3rd generation PAMAM with an ethylenediamine core, and the 4th generation PAMAM with an ethylenediamine core;

[0102] The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone;

[0103] Preferably, the weight average molecular weight of the dendritic macromolecule is 4000-85000, the intrinsic viscosity at 30°C is 0.025-0.045 dL / g, and the kinematic viscosity is 10-10000 mm 2 / s, and the degree of branching is 4000-18000 (Mw). In the present disclosure, the degree of branching of the dendrimer is measured by weight average molecular weight (Mw).

[0104] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.

[0105] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.

[0106] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.

[0107] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0108] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite catalytic material is 1 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.

[0109] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.

[0110] The present disclosure will be further described below using embodiments.

[0111] In the present disclosure, the infrared hydroxyl test steps are as follows: pressing the sample into a self-supporting sheet; placing the sample sheet into a reaction cell under high vacuum of 1.0×10 -3Pa, purified at 550 °C for 2 hours; the temperature was reduced to 150 °C and the infrared spectrum was measured by NICOLET 6700 with a wave number range of 400-4000 cm -1 .

[0112] The X-ray diffraction (XRD) crystal phase diagram of the sample was determined on a Siemens D5005 X-ray diffractometer, the radiation source was Kα (Cu), and the test range 2θ was 0.5° to 70°.

[0113] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.

[0114] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.

[0115] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.

[0116] In the following examples, among the dendritic macromolecules used, PAMAM is a polyamide-amine type dendritic macromolecule purchased from Inokai, with a molecular weight of 9858 for PAMAM (ethylenediamine core, 2nd generation), an intrinsic viscosity of 0.037 dL / g at 30°C, and a degree of branching of 4300 (Mw); PAMAM (ethylenediamine core, 3rd generation) has a molecular weight of 9858, an intrinsic viscosity of 0.035 dL / g at 30°C, and a degree of branching of 5200 (Mw); PAMAM (ethylenediamine core, 4th generation) has a molecular weight of 26000, an intrinsic viscosity of 0.031 dL / g at 30°C, and a degree of branching of 16000 (Mw); polyarylether macromolecules purchased from Inokai, polyarylether nitrile molecular weight of 83000. The weight average molecular weight and degree of branching of the dendritic macromolecules in the present disclosure are obtained through reagent labels; the intrinsic viscosity at 30°C is obtained by Ubbelohde viscometer and conventional measurement methods.

[0117] Example 1

[0118] (1) 1.6 g of a 25.05 wt % tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol) and 52.8 g of water (3 mol) were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;

[0119] (2) 0.03 g of cobalt nitrate hexahydrate (0.1 mmol) and 0.18 g (0.01 mol) of water were stirred evenly, and then 0.05 g of PAMAM (ethylenediamine core, second generation) was added, and the aqueous solution of cobalt was mixed with the hydrolyzed solution of silicon obtained in step (1);

[0120] (3) adding 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) to the mixture of step (2) and stirring for 0.5 hour;

[0121] (4) The mixture obtained in step (3) was transferred to a stainless steel closed reactor and crystallized at 175° C. for 24 h to obtain a sample. The obtained sample was filtered, washed, dried at 110° C. for 6 h, and then calcined in a muffle furnace for 6 h to obtain a metal nanoparticle and molecular sieve composite catalytic material product, which was recorded as CAT-1. Its infrared hydroxyl spectrum is shown in FIG. Figure 1 As shown, among them, 3734cm -1 The peak at represents the relative intensity of the terminal silanol group; its BET specific surface area, total pore volume, micropore volume and mesopore volume are listed in Table 2. The XRD pattern of the product is shown in Figure 2 As shown in Figure 1, the XRD pattern proves that the obtained product has an MFI molecular sieve structure. The SEM image of the product is shown in Figure 1. Figure 3 As shown, it can be seen that the obtained products have regular shapes and uniform sizes.

[0122] The BET specific surface area, total pore volume, micropore volume, mesopore volume of CAT-1 and the average particle size of metal nanoparticles in the composite catalytic material are listed in Table 2.

[0123] Preparation Example

[0124] Used to prepare pure all-silicon molecular sieve corresponding to CAT-1. Prepare the corresponding product according to the method of the corresponding Example 1, except that cobalt nitrate hexahydrate and dendritic macromolecules are not added. Other conditions and operations refer to Example 1.

[0125] The infrared hydroxyl spectrum of the pure all-silicon molecular sieve is 3730-3740cm -1 The peak intensity of the highest peak in the range is 0.048.

[0126] Comparative Example 1

[0127] This comparative example was prepared according to the method of Example 1, except that no silanization agent was added. The proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1. The prepared product is recorded as sample D-1.

[0128] Comparative Example 2

[0129] This comparative example was prepared according to patent CN 111847471 A.

[0130] Under stirring conditions, tetraethyl orthosilicate, tetrapropylammonium hydroxide, cobalt nitrate hexahydrate and deionized water are mixed to obtain a first mixture with a molar ratio of SiO2: structure directing agent: Co: H2O = 1: 0.2: 0.001: 30; then PHAPTMS is added to the above first mixture at a molar ratio of SiO2: silanization agent = 1: 0.025, and after stirring evenly, the obtained second mixture is transferred to a pressure-resistant stainless steel reactor; under stirring conditions, it is heated to 170°C and crystallized under autogenous pressure for 8 hours. After the stainless steel pressure-resistant reactor is cooled to room temperature, the crystallized product is recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous molecular sieve encapsulating cobalt. The obtained product is recorded as D-2.

[0131] Comparative Example 3

[0132] This comparative example was prepared according to the method of Ning Wang et al. (JACS, 2016, Vol. 138, pp. 7484-7487).

[0133] First, deionized water was mixed with 13g TPAOH solution and stirred continuously for 10 minutes, and then 8.32g ethyl orthosilicate (0.04mol) was added. After continuous stirring for 6 hours, the mixture became clear after complete hydrolysis. 0.052g cobalt nitrate hexahydrate (0.18mmol, the molar ratio of metal cobalt to silicon source was 0.0045) was dissolved in a mixture of 0.3mL ethylenediamine and 3mL water to prepare [Pd(NH2CH2CH2NH2)2]Cl2 solution, and then the resulting solution was added dropwise to the above mixture and stirred for 30min without precipitation. The reaction mixture was transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner and static crystallization was performed at 170°C in a conventional oven for 4 days. The solid product was centrifuged, washed with water and ethanol several times, dried in an oven at 80°C overnight, roasted in an air atmosphere at 550°C for 8 hours, and finally reduced with hydrogen to obtain the product. The obtained product was recorded as D-3.

[0134] Embodiment 2 to Embodiment 9

[0135] The corresponding products CAT-2 to CAT-9 were prepared according to the method of Example 1, and their proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations are similar to those of Example 1.

[0136] Example 10

[0137] The cobalt-containing multi-level porous β molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent. The template agent used was tetraethylammonium hydroxide (TEAOH). The ratio, synthesis conditions and results are listed in Table 1. The obtained product was recorded as CAT-10.

[0138] Embodiment 11

[0139] The cobalt-containing multi-level porous MEL molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent. The template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product is recorded as CAT-11.

[0140] Example 12

[0141] The corresponding product was prepared according to the method of Example 1, and its proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1. The obtained product is recorded as CAT-12.

[0142] The hydrothermal crystallization temperature is 120°C and the hydrothermal crystallization time is 6 days; the calcination temperature is 850°C and the calcination time is 9 hours.

[0143] The preparation methods of the pure all-silicon molecular sieves corresponding to the composite catalytic materials prepared in Examples 2 to 12 refer to the preparation method in Example 1, except that no metal element precursors and dendritic macromolecules are added during the preparation of the corresponding composite catalytic materials.

[0144] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of metal nanoparticles in the composite catalytic material of the products obtained in the above examples and comparative examples are listed in Table 2 below.

[0145] Table 1

[0146]

[0147]

[0148] In m / 10×c*, m represents the mass of the dendrimer and c represents the amount of the silicon source in terms of SiO2.

[0149] In Table 1, the cobalt nitrate used is cobalt nitrate hexahydrate; TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane); EDTA is ethylenediaminetetraacetic acid; PAMAM is polyamide-amine macromolecule. The reagents used in the present disclosure can be obtained through conventional purchasing channels.

[0150] Table 2

[0151]

[0152] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.

[0153] According to Table 2, compared with D-1 prepared in Comparative Example 1 (without adding silanizing agent and structural filler) and D-3 prepared in Comparative Example 3 (without adding silanizing agent), silanizing agents and structural fillers are added during the preparation process of Examples 1 to 12 of the present disclosure, and the obtained products CAT-1 to CAT-12 have higher mesopore volumes, indicating that the method provided in the present disclosure can effectively expand the pores of the molecular sieve.

[0154] Compared with D-2 prepared in Comparative Example 2 (without adding dendritic macromolecules), the metal nanoparticles CAT-1 to CAT-12 prepared in the present disclosure have a smaller average particle size, indicating that the CAT-1 to CAT-12 nanoparticles have a lower degree of aggregation and a higher degree of dispersion.

[0155] Test Case

[0156] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0157] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.

[0158] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):

[0159]

[0160]

[0161]

[0162] The samples prepared in the above examples and comparative examples were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde: cyclooctene = 3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1 MPa, the amount of cyclooctene was 1 mmol, the amount of catalyst was 50 mg, and the amount of solvent acetonitrile was 2.5 mL. The reaction was stable at 25°C for 6 hours, and samples were taken for analysis. The results are shown in Table 3.

[0163] Table 3

[0164]

[0165] According to the data in Table 3, compared with D-1 to D-3 prepared in comparative examples 1-3, the I0 of the composite catalytic materials CAT-1 to CAT-12 prepared in embodiments 1 to 12 of the present disclosure is 0.30 to 0.98, which has higher catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde, and higher cyclooctene conversion rate and epoxycyclooctene selectivity.

[0166] Furthermore, by comparing CAT-1 to CAT-11 with CAT-12, it can be seen that the I0 of CAT-1 to CAT-11 is between 0.35 and 0.98, and the cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity of CAT-1 to CAT-11 are higher.

[0167] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0168] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0169] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A metal nanoparticle and molecular sieve composite catalytic material, characterized in that: It comprises an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; The composite catalytic material has the following IR-OH characteristics: The wave number in the IR-OH spectrum of the composite catalyst material is 3730-3740cm -1 The peak intensity of the highest peak in the range is recorded as I1; the wave number in the IR-OH spectrum of pure all-silicon molecular sieve is 3730~3740cm -1 The peak intensity of the highest peak in the range is recorded as I2. I0 defined by the following formula (1) is any value between 0.35 and 0.98; I0= I1 / I2 (1); The metal nanoparticle and molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments; In step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms; The dendritic macromolecule is selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules.

2. The composite catalytic material according to claim 1, characterized in that: The all-silicon molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.

3. The composite catalytic material according to claim 2, characterized in that: The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the group consisting of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.

4. The composite catalytic material according to claim 3, characterized in that: The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, the MEL structure molecular sieve and the BEA structure molecular sieve.

5. The composite catalytic material according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.2):

1.

6. The composite catalytic material according to claim 5, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.16):

1.

7. The composite catalytic material according to claim 1, characterized in that: The BET specific surface area of ​​the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.2~0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~6nm.

8. The composite catalytic material according to claim 1, characterized in that: In step S1, the molar ratio of silicon source calculated as SiO2: template: water: metal M element: silanization agent is 1: (0.005-1): (10-80): (0.001-0.2): (0.025-0.4); the ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01-3):

1.

9. The composite catalytic material according to claim 8, characterized in that: In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.005-1): (10-80): (0.001-0.16): (0.025-0.3).

10. The composite catalytic material according to claim 1, characterized in that: Step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. adding dendritic macromolecules to the aqueous solution of the metal M precursor, and mixing them to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.

11. The composite catalytic material according to claim 10, characterized in that: The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.

12. The composite catalytic material according to claim 1, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.

13. The composite catalytic material according to claim 12, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.

14. The composite catalytic material according to claim 13, characterized in that: The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.

15. The composite catalytic material according to claim 14, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.

16. The composite catalytic material according to claim 15, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.

17. The composite catalytic material according to claim 16, characterized in that: The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

18. The composite catalytic material according to claim 1, characterized in that: In step S1, the template agent is an organic base.

19. The composite catalytic material according to claim 18, characterized in that: The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.

20. The composite catalytic material according to claim 19, characterized in that The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.

21. The composite catalytic material according to claim 20, characterized in that: In formula (B), R1, R2, R3 and R4 are each selected from one of a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.

22. The composite catalytic material according to claim 21, characterized in that In formula (B), R1, R2, R3 and R4 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

23. The composite catalytic material according to claim 1, characterized in that: The molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

24. The composite catalytic material according to claim 10, characterized in that: In step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain a hydrolyzed solution of the silicon; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.

25. The composite catalytic material according to claim 24, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.

26. The composite catalytic material according to claim 1, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M.

27. The composite catalytic material according to claim 26, characterized in that The metal M precursor is a water-soluble inorganic salt of metal M.

28. The composite catalytic material according to claim 10, characterized in that: The molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).

29. The composite catalytic material according to claim 1, characterized in that: The silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

30. The composite catalytic material according to claim 29, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

31. The composite catalytic material according to claim 1, characterized in that In step S1, the polyamidoamine macromolecule is selected from one or more of the second generation PAMAM with an ethylenediamine core, the third generation PAMAM with an ethylenediamine core, and the fourth generation PAMAM with an ethylenediamine core; The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone.

32. The composite catalytic material according to claim 1, characterized in that The dendritic macromolecule has a weight average molecular weight of 4000-85000, an intrinsic viscosity of 0.025-0.045 dL / g at 30° C., and a branching degree of 4000-18000.

33. The composite catalytic material according to claim 1, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.

34. The composite catalytic material according to claim 33, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.

35. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 34 in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins.

36. The use according to claim 35, characterized in that The use includes the use of the metal nanoparticles and molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.