A composite catalytic material containing framework heteroatom molecular sieve and its preparation method and application
By introducing heteroatom precursors and metal precursors during the synthesis process of molecular sieves, combined with polyhydroxyl additives and silanization reagents, a hierarchical porous structure of metal oxide nanoparticles and molecular sieve composite catalytic materials is formed, which solves the problem of metal nanoparticles within the molecular sieve framework. The high dispersion and synergistic catalysis of particles improve the catalytic activity and reactivity.
Patent Information
- Application Number
- CN202111422410.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-11-26
AI Technical Summary
It is difficult to simultaneously achieve high dispersion and synergistic catalysis of metal nanoparticles within the molecular sieve framework through one preparation method with the existing technology, and the micropores of the molecular sieve limit the contact of macromolecular reactants, resulting in catalyst deactivation.
A composite catalytic material of metal oxide nanoparticles and molecular sieves is used. By introducing heteroatom precursors and metal element precursors during the molecular sieve synthesis process, combined with polyhydroxyl additives and silanization reagents, a hierarchical porous structure and highly dispersed catalytic material are formed. Metal nanoparticles achieve synergistic catalysis between framework heteroatoms and metal nanoparticles.
The uniform dispersion of metal nanoparticles in the hierarchical pore structure molecular sieve is achieved, which improves the catalytic activity and reaction activity, prolongs the service life of the catalyst, and significantly improves the catalytic activity in the aldehyde/alkene co-oxidation reaction.
Smart Images

Figure CN116174017B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a composite catalytic material containing a framework heteroatom molecular sieve, and a preparation method and application thereof. Background Art
[0002] MFI molecular sieves have the advantages of adjustable surface acidity, shape-selective catalysis, and good hydrothermal stability, making them ideal carriers for loading metal active centers. However, the micropores of molecular sieves often limit the accessibility of larger reactant molecules to the internal catalytic centers, and the inactivation of catalysts due to the inability of large molecules to pass through the micropores has become the main problem restricting the application of such materials. For this reason, people have designed and synthesized multi-level pore MFI molecular sieves, that is, in the same system, they contain both micropores, mesopores, and even macropores. The diversity of molecular sieve pore sizes increases the speed at which reactants and products pass through the internal pores, increases the contact opportunities between the catalytic center and the reactants, and thus improves the ability to catalytically activate large molecular reactants; at the same time, multi-level pores can remove products and by-products by providing a faster transfer path, thereby extending the service life of the catalyst. On the other hand, MFI molecular sieves are often used to prepare acidic metal bifunctional catalysts. During the reaction, the acidic sites of the molecular sieves synergistically catalyze with the loaded metal species, resulting in significant changes in catalytic activity and product selectivity. In recent years, metal-doped MFI molecular sieves have attracted much attention both in the fields of materials chemistry and catalytic chemistry.
[0003] Direct hydrothermal synthesis is a common way to introduce metals into molecular sieves. It generally refers to the direct introduction of metal precursors during the crystallization process of molecular sieves. During the hydrothermal crystallization process, the metal precursors can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structural units, the metal nanoparticles are evenly embedded in the molecular sieve framework. Since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursors are very easy to form hydroxide precipitation. To solve this problem, the precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.). In addition to preventing coagulation, the complexing agent can also play the role of isolation and dispersion, which helps to form highly dispersed metal nanoparticles. Highly dispersed metal nanoparticles help to inhibit the sintering of metals at high temperatures.
[0004] Wang Baorong et al. (CN 111847471A) prepared a multi-level porous molecular sieve encapsulating active metals by introducing a silanization agent in a direct hydrothermal synthesis method. However, since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursor is very likely to form a hydroxide precipitate. This problem has not been solved. Precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.). For example, Wang et al. used ethylenediamine ligands and PdCl2 to form [Pd(NH2CH2CH2NH2)]Cl2 complex precursors, and then directly synthesized silicalite-1 molecular sieves (Pd@silicalite-1) that embedded uniformly dispersed Pd nanoparticles through a hydrothermal crystallization method.
[0005] The action of several catalysts or multifunctional catalysts, as well as the action of multi-component catalysts that form composite active centers that are conducive to the reaction by the synergistic action of the components, is called synergistic catalysis. If the catalytic action of the metal sites on the molecular sieve framework and the metal sites (nanoparticles) that are difficult to enter the framework but are in the molecular sieve pores are exerted at the same time, so that they play a synergistic catalytic effect, then a good catalytic effect will be achieved.
[0006] In summary, the prior art highly disperses metal nanoparticles in the molecular sieve crystals by complexing metal precursors with organic ligands and then introducing them into the molecular sieve hydrothermal crystallization process, and expands the pores by introducing silanization agents into the molecular sieve synthesis process. However, the prior art cannot achieve the above two effects at the same time through a single preparation method; nor can it achieve the synergistic catalytic effect of the framework heteroatom sites and the metal nanoparticles in the molecular sieve pores. Summary of the invention
[0007] The purpose of the present disclosure is to provide a composite catalytic material containing a framework heteroatom molecular sieve, and a preparation method and application thereof. The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal nanoparticles have uniform particle size and are evenly dispersed in the framework heteroatom molecular sieve crystal with a multi-level pore structure, and play a synergistic catalytic role with the heteroatoms in the framework.
[0008] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium;
[0009] The composite catalytic material has the following 29 Si NMR characteristics:
[0010] The composite catalytic material 29 The intensity at the chemical shift of -103 ppm in the Si NMR spectrum is recorded as Q3, and the intensity at the chemical shift of -113 ppm is recorded as Q4;
[0011] Q0 defined by the following formula (1) is any value between 0.05 and 0.1;
[0012] Q0=Q3 / Q4 formula (1).
[0013] Optionally, the Q0 is any value between 0.05 and 0.09.
[0014] Optionally, the framework heteroatom molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0015] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0016] Optionally, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1, preferably (0.005-0.04):1;
[0017] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.001-0.15):1.
[0018] Optionally, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the mesopore volume is 0.2-0.65mL / g, the micropore volume is 0.1-0.19mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-10nm.
[0019] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:
[0020] S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a polyhydroxy auxiliary agent and a silanization agent to obtain a reaction mixture;
[0021] S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments;
[0022] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; the silanization agent contains at least one coordination group complexed with the metal element M; and the polyhydroxy auxiliary agent is a compound containing at least two hydroxyl groups.
[0023] Optionally, in step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the polyhydroxy auxiliary agent: the silanization agent is 1: (0.005~1): (0.001~0.05): (10~80): (0.001~0.2): (0.5~5): (0.015~0.4); preferably 1: (0.005~1): (0.005~0.04): (10~80): (0.001~0.15): (0.5~5): (0.015~0.3).
[0024] Optionally, step S1 includes the following steps:
[0025] a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution;
[0026] b. Adding the polyhydroxy auxiliary agent to the aqueous solution of the metal M precursor to obtain a first mixed material; mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material;
[0027] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;
[0028] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
[0029] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0030] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0031]
[0032] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , Rb , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0033] Optionally, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0034] wherein R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from one of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group and a tert-butyl group;
[0035] Further preferably, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0036] The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0037] The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0038] Optionally, in step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain the hydrolysis solution;
[0039] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0040] Optionally, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one selected from chlorides, nitrates and sulfates of heteroatom element Q; the inorganic skeleton heteroatom precursor is an organic acid ester containing heteroatom element Q, selected from at least one of the structures represented by the following formula (C):
[0041]
[0042] wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R5, R6, R7 and R8 are independently selected from a straight-chain alkyl group having 2 to 4 carbon atoms and a branched-chain alkyl group having 2 to 4 carbon atoms;
[0043] Optionally, R5, R6, R7 and R8 are each independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl; preferably, each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl;
[0044] Preferably, when the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is boron, the skeleton heteroatom precursor is selected from one or more of boric acid and borate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is aluminum, the skeleton heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; when the skeleton heteroatom is phosphorus, the skeleton heteroatom precursor is selected from one or more of orthophosphoric acid, triethyl phosphoric acid and metaphosphate; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.
[0045] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal M precursor is a water-soluble inorganic salt of the metal element M;
[0046] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0047] Preferably, the metal M precursor is an aqueous solution of the metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0048] Optionally, in step S1, the polyhydroxy auxiliary agent is selected from one or more of polyols and sugar substances;
[0049] Preferably, the polyol comprises one or more of ethylene glycol, glycerol, pentaerythritol, 1,2-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, diethylene glycol and polyether polyol; wherein the polyether polyol comprises one or more of propylene glycol polyether, trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol; the weight average molecular weight of the propylene glycol polyether is 800-2000, and the weight average molecular weight of the trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol is independently 400-4000;
[0050] The sugar substances include one or more of glucose, sucrose, fructose, starch and cellulose.
[0051] Optionally, in step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the carbon number of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer from 1 to 18, and the carbon number of the aromatic group is any integer from 6 to 18;
[0052] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0053] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;
[0054] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0055] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0056] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0057] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The present disclosure introduces a heteroatom precursor in the molecular sieve crystallization synthesis process, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present disclosure also introduces a metal element precursor, a polyhydroxy auxiliary agent and a silanization agent into the reaction mixture, and the molecular sieve of the prepared composite catalytic material has a multi-level pore structure and a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have a uniform particle size and are evenly dispersed in the crystal of the multi-level pore heteroatom framework molecular sieve (for example, in the mesoporous channel); wherein the metal element and the heteroatom in the framework can play a synergistic catalytic role. The Q0 of the composite catalytic material provided by the present disclosure is any value between 0.05 and 0.1, and has a high catalytic activity in the co-oxidation reaction of aldehydes / olefins.
[0058] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0060] Figure 1 The product obtained in Example 1 is prepared 29 Si NMR spectrum.
[0061] Figure 2 This is the UV-Vis graph of the product prepared in Example 1.
[0062] Figure 3 The XRD spectrum of the product prepared in Example 1 is shown.
[0063] Figure 4 This is the SEM image of the product prepared in Example 1. DETAILED DESCRIPTION
[0064] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0065] The inventors of the present disclosure surprisingly discovered through a large number of experiments that heteroatom precursors, metal M precursors, polyhydroxy auxiliary agents and silanization agents (containing at least one coordination group complexed with the metal element M) are introduced into the reaction raw materials for crystallization synthesis of molecular sieves, and after hydrothermal crystallization treatment and calcination treatment, heteroatoms can be introduced into the molecular sieve framework, and the skeleton heteroatom molecular sieve of the composite catalytic material obtained has a multi-level pore structure (micropores and mesopores) and a large specific surface area and pore volume, the metal oxide nanoparticles have a high uniformity in particle size and can be evenly dispersed in the pores of the skeleton heteroatom molecular sieve, and a certain amount of metal M nanoparticles will also exist on the surface of the pores; the heteroatom metal sites on the molecular sieve framework and the metal sites (nanoparticles) of the metal element M in the pores can also play a synergistic catalytic effect, further improving the catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins.
[0066] The inventors have found through further research that the composite catalytic material 29In the Si NMR spectrum, the ratio of the peak intensity between the highest peak with a chemical shift of -103ppm (representing the terminal silanol group) and the highest peak with a chemical shift of -113ppm (representing four-matched silicon) is related to the catalytic activity of the composite catalytic material in the co-oxidation reaction of aldehyde / olefin. When the ratio Q0 (Q0=Q3 / Q4) of the peak intensity of the highest peak with a chemical shift of -103ppm (denoted as Q3) and the peak intensity of the highest peak with a chemical shift of -113ppm (denoted as Q4) is any value between 0.05 and 0.1, the composite catalytic material can obtain a higher catalytic activity and effectively improve the cyclooctene conversion rate and the epoxycyclooctene selectivity.
[0067] The first aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; the composite catalytic material has the following 29 Si NMR characteristics: The composite catalytic material 29 The intensity at the chemical shift of -103 ppm in the Si NMR spectrum is recorded as Q3, and the intensity at the chemical shift of -113 ppm is recorded as Q4;
[0068] Q0 defined by the following formula (1) is any value between 0.05 and 0.1; Q0 = Q3 / Q4 (1).
[0069] The present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves, wherein the molecular sieve of the composite catalytic material has a multi-level pore structure and a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore heteroatom framework molecular sieve. There is an obvious interaction between the metal elements of the metal oxide particles and the heteroatoms in the framework. After the heteroatoms are introduced into the molecular sieve framework, the two metal sites in the composite catalytic material can play a synergistic catalytic role. Q0 is any value between 0.05 and 0.1, and has a high catalytic activity in the co-oxidation reaction of aldehydes / olefins.
[0070] In this disclosure 29 The peak with a chemical shift of -103 ppm in the Si NMR spectrum represents terminal silanol groups, and its chemical structure is shown in the following formula (I); the peak with a chemical shift of -113 ppm represents tetra-matched silicon, and its chemical structure is shown in the following formula (I I). In the present disclosure, Q0 is used to represent the proportion of terminal silanol groups in the total silicon species.
[0071]
[0072] In a preferred embodiment, Q0 is any value between 0.05 and 0.09. When Q0 of the composite catalyst material is within this range, the composite catalyst material has higher catalytic activity, cyclooctene conversion rate and epoxycyclooctene selectivity.
[0073] In one embodiment, the skeleton heteroatom molecular sieve in the composite catalytic material is one or more of MFI structure molecular sieve (such as S-1), MEL structure molecular sieve (such as S-2), BEA structure molecular sieve (such as Beta), MWW structure molecular sieve (such as MCM-22), two-dimensional hexagonal structure molecular sieve (such as MCM-41, SBA-15), MOR structure molecular sieve (such as MOR), TUN structure molecular sieve (such as TUN) and silicon molecular sieves of other structures (such as ZSM-48, MCM-48); preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve, such as the silicon molecular sieve is one of S-1, S-2 and Beta; further preferably, it is an MFI structure molecular sieve, such as S-1.
[0074] In one embodiment, the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0075] In one embodiment, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1, preferably (0.005-0.04):1;
[0076] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.001-0.15):1.
[0077] In one embodiment, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, preferably 420 to 750 m 2 / g; total pore volume is 0.3-0.65mL / g, preferably 0.35-0.6mL / g; micropore volume is 0.1-0.19mL / g, preferably 0.1-0.18mL / g, mesopore volume is 0.2-0.19mL / g, preferably 0.21-0.41mL / g, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-10nm, preferably 0.9-9nm. The composite catalytic material disclosed in the present invention has a multi-level pore structure, which is conducive to catalyzing reaction substrates of different sizes, especially catalyzing the reaction of macromolecular substrates.
[0078] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising the following steps:
[0079] S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a polyhydroxy auxiliary agent and a silanization agent to obtain a reaction mixture;
[0080] S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments;
[0081] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; the silanization agent contains at least one coordination group complexed with the metal element M; and the polyhydroxy auxiliary agent is a compound containing at least two hydroxyl groups.
[0082] The present disclosure introduces heteroatom precursors into the reaction mixture for molecular sieve synthesis, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present disclosure also introduces metal element precursors, polyhydroxy auxiliary agents and silanization agents into the reaction mixture, wherein the polyhydroxy auxiliary agents can be complexed with metal M ions to fix and disperse the metal elements; and the coordination group of the silanization agent complexes the metal to fix and disperse the metal elements, and the supporting layer of the alkyl chain has a pore expansion effect; so that a skeleton heteroatom molecular sieve with a multi-level pore structure is finally prepared, and the metal M oxide nanoparticles can also be uniformly dispersed in the mesoporous channels of the multi-level pore skeleton heteroatom molecular sieve.
[0083] In one embodiment, in step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the polyhydroxy auxiliary agent: the silanization agent is 1: (0.005-1): (0.001-0.05): (10-80): (0.001-0.2): (0.5-5): (0.015-0.4); preferably 1: (0.005-1): (0.005-0.04): (10-80): (0.001-0.15): (0.5-5): (0.015-0.3).
[0084] Specifically, the water used in step S1 can be water commonly used in synthesizing molecular sieves. In order to avoid the introduction of heteroatoms, deionized water is preferred.
[0085] In a preferred embodiment, step S1 comprises the following steps:
[0086] a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution;
[0087] b. Adding the polyhydroxy auxiliary agent to the aqueous solution of the metal M precursor to obtain a first mixed material; mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material;
[0088] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;
[0089] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
[0090] In one embodiment, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0091] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0092]
[0093] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
[0094] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0095] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.
[0096] In a further preferred embodiment, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0097] Wherein R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0098] In a preferred embodiment, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0099] In another preferred embodiment, the molecular sieve in the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0100] In another preferred embodiment, the molecular sieve in the composite catalyst material is a Beta molecular sieve, and the template is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0101] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution;
[0102] The conditions for the hydrolysis and alcohol removal treatment include: stirring hydrolysis at 0-95°C for 2-10 hours; preferably stirring hydrolysis at 50-95°C for 2-8 hours; wherein the hydrolysis and alcohol removal treatment makes the mass content of alcohol produced by hydrolysis of the organosilicon source in the hydrolysis solution less than 10 ppm.
[0103] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal element (such as a compound containing the metal element and / or a metal element) can achieve the purpose of the present disclosure.
[0104] In one embodiment, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one of a chloride, a nitrate or a sulfate of a heteroatom element; the inorganic skeleton heteroatom precursor is an organic acid ester containing a heteroatom element, selected from at least one of the structures represented by the following formula (C):
[0105]
[0106] wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R5, R6, R7 and R8 are independently selected from a straight-chain alkyl group having 2 to 4 carbon atoms and a branched-chain alkyl group having 2 to 4 carbon atoms;
[0107] Optionally, R5, R6, R7 and R8 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl; preferably, they are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
[0108] In an optional embodiment, the skeleton heteroatom is titanium, and the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; in an optional embodiment, the skeleton heteroatom is boron, and the skeleton heteroatom precursor is selected from one or more of boric acid and borate; in an optional embodiment, the skeleton heteroatom is tin, and the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide. In one optional embodiment, the framework heteroatom is aluminum, and the framework heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; in one optional embodiment, the framework heteroatom is phosphorus, and the framework heteroatom precursor is selected from one or more of orthophosphoric acid, triethylphosphoric acid and metaphosphate; in one optional embodiment, the framework heteroatom is germanium, and the framework heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide (such as ethanol germanium, isopropoxide germanium), germanium chloride and sodium germanate.
[0109] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal M precursor is a water-soluble inorganic salt of the metal element M;
[0110] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0111] Preferably, the metal M precursor is an aqueous solution of the metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0112] In one embodiment, in step S1, the polyhydroxy auxiliary agent is selected from one or more of polyols and sugar substances;
[0113] Preferably, the polyol comprises one or more of ethylene glycol, glycerol, pentaerythritol, 1,2-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, diethylene glycol and polyether polyol; wherein the polyether polyol comprises one or more of propylene glycol polyether, trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol; the weight average molecular weight of the propylene glycol polyether is 800-2000, and the weight average molecular weight of the trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol is independently 400-4000;
[0114] The sugar substances include one or more of glucose, sucrose, fructose, starch and cellulose.
[0115] In one embodiment, in step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer in the range of 1 to 18, preferably any integer in the range of 1 to 12; the number of carbon atoms of the aromatic group can be any integer in the range of 6 to 18, preferably any integer in the range of 6 to 12.
[0116] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0117] In the present disclosure, different silanization agents can be selected for different metal elements M. For example, when the metal element M is Co, the silanization agent is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; when the metal element M is Au or Pt, the silanization agent is at least one of 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.
[0118] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.
[0119] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.
[0120] The third aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves prepared according to the method described in the second aspect of the present disclosure.
[0121] The fourth aspect of the present disclosure provides the use of the metal oxide nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0122] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite catalytic material is 5 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; the oxygen pressure is 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.
[0123] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.
[0124] In the present disclosure, the samples were characterized by Raman spectrometer on LabRAMHR UV-NIR confocal microscope. The test conditions were: room temperature, normal pressure, laser wavelength of 532nm, and spectral acquisition range of 170-1200cm -1 .
[0125] The UV-visible diffuse reflectance spectrum (UV-vis) of the samples was measured on a SHIMADZU UV-3100 UV-visible spectrometer in the range of 400 to 4000 cm -1 .
[0126] The X-ray diffraction (XRD) crystal phase diagram of the sample was measured on a Siemens D5005 X-ray diffractometer, the radiation source was Kα (Cu), and the test range 2θ was 0.5° to 70°.
[0127] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.
[0128] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.
[0129] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0130] Example 1
[0131] (1) 1.63 g of 25.05 wt % tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol), 0.170 g of tetrabutyl titanate (0.0005 mol) and 9 g (0.5 mol) of water were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 80° C. for 3 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;
[0132] (2) 0.3 g of cobalt nitrate hexahydrate (1 mmol) and 1.8 g (0.1 mol) of water were stirred evenly, and then 0.5 mmol of ethylene glycol was added to mix the aqueous solution of cobalt with the hydrolyzed solution of silicon obtained in step (1);
[0133] (3) adding 0.56 g of N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (silane coupling agent KH-792, 0.0025 mol) to the mixture of step (2) and stirring for 0.5 hour;
[0134] (4) The mixture obtained in step (3) is transferred to a stainless steel closed reactor and crystallized at a constant temperature of 170°C for 28 hours to obtain a sample. The obtained sample is filtered and washed, dried at 120°C for 6 hours, and then calcined in a muffle furnace at 550°C for 6 hours to obtain a metal nanoparticle and molecular sieve composite catalytic material product, which is recorded as C-1.
[0135] C-1 29 Si NMR images Figure 1 The UV-Vis image of C-1 is shown in Figure 2 As shown, Figure 1 The peak at -103nm indicates the intensity of terminal silanol groups, and the peak at -113nm indicates the intensity of tetracoordinated silicon. Figure 2 The peak near 250nm in the spectrum represents titanium species. The XRD spectrum of C-1 is shown in Figure 3 As shown in Figure 2, XRD analysis shows that it has an MFI structure. The SEM spectrum of C-1 is shown in Figure 2. Figure 4 As shown, it can be seen that the products have regular shapes and uniform sizes.
[0136] The BET specific surface area, total pore volume, micropore volume, mesopore volume and the average particle size of the metal nanoparticles contained in C-1 are listed in Table 2.
[0137] Comparative Example 1
[0138] This comparative example was prepared according to the method of Example 1, except that no silanization agent was added. The proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations were similar to those of Example 1, and the obtained product was recorded as D-1.
[0139] Comparative Example 2
[0140] Under stirring conditions, tetraethyl orthosilicate, tetrapropylammonium hydroxide, tetrabutyl titanate, cobalt nitrate and deionized water were mixed and stirred at 50°C for 2 hours to obtain a first mixture with a molar ratio of SiO2: structure directing agent: TiO2: Co: H2O = 1: 0.2: 0.03: 0.01: 30; then PHAPTMS was added to the above first mixture at a molar ratio of SiO2: silanization agent = 1: 0.025, and after continuing to stir for 0.5 hours, the obtained second mixture was transferred to a pressure-resistant stainless steel reactor; under stirring conditions, it was heated to 170°C and crystallized under autogenous pressure for 8 hours. After the stainless steel pressure-resistant reactor was cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous molecular sieve encapsulating cobalt, and the obtained product was recorded as D-2.
[0141] Comparative Example 3
[0142] Under stirring conditions, tetraethyl orthosilicate, tetrapropylammonium hydroxide, tetrabutyl titanate, cobalt acetylacetonate and deionized water were mixed and stirred at 80°C for 8 hours to obtain a first mixture with a molar ratio of SiO2: structure directing agent: TiO2: Co: H2O = 1: 0.2: 0.025: 0.01: 50; then phenyltriethoxysilane was added to the above first mixture at a molar ratio of SiO2: silanization agent = 1: 0.12, and after stirring evenly, the obtained second mixture was transferred to a pressure-resistant stainless steel reactor; after continuing to stir for 2 hours, it was heated to 170°C and crystallized under autogenous pressure for 8 hours. After the stainless steel pressure-resistant reactor was cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous titanium silicon molecular sieve encapsulating cobalt, and the obtained product was recorded as D-3.
[0143] Embodiments 2 to 9
[0144] The corresponding products C-2 to C-9 were prepared according to the method of Example 1, and their proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations are similar to those of Example 1.
[0145] Example 10
[0146] In this example, a cobalt-containing multi-level porous β molecular sieve was prepared, referring to the method of Example 1, but the ratio and template agent were changed, and the template agent used was tetraethylammonium hydroxide (TEAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product was recorded as C-10.
[0147] Embodiment 11
[0148] In this example, a cobalt-containing multi-level porous MEL molecular sieve was prepared, referring to the method of Example 1, but the ratio and template agent were changed, and the template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product was recorded as C-11.
[0149] Example 12
[0150] The corresponding product was prepared according to the method of Example 1, and its ratio, synthesis conditions and results are shown in Table 1. Other conditions and operations refer to Example 1, and the obtained product is recorded as C-12. The hydrothermal crystallization temperature is 120°C, the hydrothermal crystallization time is 7 days, the calcination temperature is 850°C, and the calcination time is 9 hours.
[0151] Embodiment 13
[0152] A copper-containing nanoparticle multi-level porous MFI molecular sieve was prepared, wherein the framework heteroatom was boron, according to the method of Example 1. The proportions, synthesis conditions and results are shown in Table 1. The obtained product was recorded as C-13.
[0153] The BET specific surface area, total pore volume, micropore volume, mesopore volume of the products obtained in the above examples and comparative examples, and the average particle size of the nanoparticles in the composite catalytic material are listed in Table 2 below.
[0154] Table 1
[0155]
[0156]
[0157] In Table 1, cobalt nitrate is cobalt nitrate hexahydrate; TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane), PTES is phenyltriethoxysilane. The reagents used in the present disclosure can be obtained through conventional purchase channels.
[0158] Table 2
[0159]
[0160]
[0161] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0162] According to Table 2, compared with D-1 prepared in Comparative Example 1 (without adding silanization agent), the products C-1 to C-13 obtained by adding silanization agent in the preparation process of Examples 1 to 13 of the present disclosure have higher mesopore volumes, indicating that the method provided by the present disclosure can effectively expand the pores of the molecular sieve. In addition, the metal nanoparticles in the composite catalytic material prepared by the present disclosure have a smaller particle size, indicating that the metal nanoparticles have a small degree of aggregation and a high degree of dispersion.
[0163] Test Case
[0164] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0165] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.
[0166] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):
[0167]
[0168]
[0169]
[0170] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1MPa, the amount of cyclooctene was 1mmol, the amount of catalyst was 50mg, and the amount of solvent acetonitrile was 2.5mL. The reaction was stable at 25°C for 6 hours, and the samples were taken for analysis. The results are shown in Table 3.
[0171] Table 3
[0172]
[0173] It can be seen from Table 3 that compared with D-1 to D-3 prepared in comparative examples 1 to 3, the Q0 of the composite catalytic materials C-1 to C-13 prepared in embodiments 1 to 13 of the present disclosure is between 0.05 and 0.1. When C-1 to C-13 are used for the co-oxidation reaction of cyclooctene and isobutyraldehyde, they have higher catalytic activity and can obtain higher cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxy cyclooctene selectivity.
[0174] By comparing C-1 to C-13, it can be seen that the Q0 of the prepared composite catalytic material satisfies 0.05 to 0.09 (C-1 to C-11 and C-13), and the composite catalytic material has higher catalytic activity and can obtain higher cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxy cyclooctene selectivity.
[0175] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0176] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0177] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A metal nanoparticle and molecular sieve composite catalytic material, characterized in that: It comprises a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve, wherein the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, wherein the heteroatom element Q is selected from one or more of titanium, zirconium, tin and germanium; The composite catalytic material has the following 29 Si NMR characteristics: The composite catalytic material 29 The intensity at the chemical shift of -103 ppm in the Si NMR spectrum is recorded as Q3, and the intensity at the chemical shift of -113 ppm is recorded as Q4; Q0 defined by the following formula (1) is any value between 0.05 and 0.1; Q0=Q3 / Q4 (1); The metal nanoparticle and molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a polyhydroxy auxiliary agent and a silanization agent to obtain a reaction mixture; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments; Among them, the heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; the silanization agent contains at least one ligand complexed with the metal element M; the polyhydroxy auxiliary is a compound containing at least two hydroxyl groups; the polyhydroxy auxiliary is selected from one or more of polyols and sugar substances.
2. The composite catalytic material according to claim 1, characterized in that: The Q0 is any value between 0.05 and 0.
09.
3. The composite catalytic material according to claim 1, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.
4. The composite catalytic material according to claim 3, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of the following: MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
5. The composite catalytic material according to claim 4, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.
6. The composite catalytic material according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1; The molar ratio of metal M element to silicon element is (0.001~0.2):
1.
7. The composite catalytic material according to claim 6, characterized in that: In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.005-0.04):1; The molar ratio of metal M element to silicon element is (0.001~0.15):
1.
8. The composite catalytic material according to claim 1, characterized in that: The BET specific surface area of the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the mesopore volume is 0.2~0.65mL / g, the micropore volume is 0.1~0.19mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~10nm.
9. The composite catalytic material according to claim 1, characterized in that: In step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the polyhydroxy auxiliary agent: the silanization agent is 1: (0.005~1): (0.001~0.05): (10~80): (0.001~0.2): (0.5~5): (0.015~0.4).
10. The composite catalytic material according to claim 9, characterized in that: In step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the polyhydroxy auxiliary agent: the silanization agent is 1: (0.005~1): (0.005~0.04): (10~80): (0.001~0.15): (0.5~5): (0.015~0.3).
11. The composite catalytic material according to claim 1, characterized in that: Step S1 includes the following steps: a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution; b. adding the polyhydroxy auxiliary agent to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.
12. The composite catalytic material according to claim 11, characterized in that: The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
13. The composite catalytic material according to claim 1, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
14. The composite catalytic material according to claim 13, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
15. The composite catalytic material according to claim 14, characterized in that: The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
16. The composite catalytic material according to claim 15, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
17. The composite catalytic material according to claim 16, characterized in that: The R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
18. The composite catalytic material according to claim 17, characterized in that: The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
19. The composite catalytic material according to claim 1, characterized in that: The template agent is an organic base.
20. The composite catalytic material according to claim 19, characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
21. The composite catalytic material according to claim 20, characterized in that: The template is selected from at least one of the quaternary ammonium bases having the structure shown in the following formula (B): (B); wherein R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.
22. The composite catalytic material according to claim 21, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.
23. The composite catalytic material according to claim 22, characterized in that: The R1, R2, R3 and R4 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
24. The composite catalytic material according to claim 1, characterized in that The molecular sieve in the composite catalyst material is an MFI molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
25. The composite catalytic material according to claim 11, characterized in that: In step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
26. The composite catalytic material according to claim 25, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
27. The composite catalytic material according to claim 1, characterized in that In step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one selected from chlorides, nitrates and sulfates of heteroatom element Q; the organic skeleton heteroatom precursor is an organic acid ester containing heteroatom element Q, selected from at least one of the structures shown in the following formula (C): (C); wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms.
28. The composite catalytic material according to claim 27, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms.
29. The composite catalytic material according to claim 28, characterized in that The R5, R6, R7 and R8 are independently selected from a straight chain alkyl group having 2 to 4 carbon atoms and a branched chain alkyl group having 2 to 4 carbon atoms.
30. The composite catalytic material according to claim 27, characterized in that The R5, R6, R7 and R8 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl.
31. The composite catalytic material according to claim 30, characterized in that The R5, R6, R7 and R8 are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
32. The composite catalytic material according to claim 1, characterized in that When the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.
33. The composite catalytic material according to claim 1, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M.
34. The composite catalytic material according to claim 33, characterized in that The metal M precursor is a water-soluble inorganic salt of the metal element M.
35. The composite catalytic material according to claim 11, characterized in that The molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).
36. The composite catalytic material according to claim 1, characterized in that In the polyhydroxy auxiliary agent of step S1, the polyol includes one or more of ethylene glycol, glycerol, pentaerythritol, 1,2-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, diethylene glycol and polyether polyol; wherein the polyether polyol includes one or more of propylene glycol polyether, trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol; the weight average molecular weight of the propylene glycol polyether is 800-2000, and the weight average molecular weight of the trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol is independently 400-4000; The sugar substances include one or more of glucose, sucrose, fructose, starch and cellulose.
37. The composite catalytic material according to claim 1, characterized in that In step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amino group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amino group is independently selected from any integer in the range of 1 to 18, and the number of carbon atoms of the aromatic group is any integer in the range of 6 to 18.
38. The composite catalytic material according to claim 37, characterized in that The silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
39. The composite catalytic material according to claim 38, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
40. The composite catalytic material according to claim 1, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
41. The composite catalytic material according to claim 40, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.
42. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 41 in catalyzing the co-oxidation reaction of aldehydes and olefins.
43. The use according to claim 42, characterized in that The use includes use of the metal nanoparticles and the molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
Citation Information
Patent Citations
Hierarchical pore titanium silicalite molecular sieve for packaging active metal and preparation method thereof
CN111847471A
High-dispersion dual-functional catalyst for hydrogenating and deoxidizing phenol and preparation method of catalyst
CN102698788A
All-silicon molecular sieve and synthetic method thereof
CN104556087A