A composite catalytic material containing metal elements and molecular sieves, and preparation method and application thereof
By adding metal precursors, silanization reagents and peroxides during the synthesis process of molecular sieves, composite catalytic materials of metal nanoparticles and molecular sieves are prepared, which solves the problem of insufficient catalytic activity in the existing technology, especially in macromolecular reactions. Improved catalytic activity.
Patent Information
- Application Number
- CN202111424565.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-11-26
AI Technical Summary
It is difficult to realize molecular sieve catalysts with highly dispersed metal nanoparticles and hierarchical pore structures at the same time using existing technology, resulting in insufficient catalytic activity, especially poor performance in macromolecular reactions.
By simultaneously adding metal precursors, silanization reagents and peroxides during the synthesis process of molecular sieves, and performing hydrothermal crystallization and roasting treatments, composite catalytic materials of metal nanoparticles and molecular sieves are prepared to ensure that metal oxide nanoparticles are evenly dispersed in multiple materials. hierarchical pore molecular sieves and improve catalytic activity.
The macromolecule reaction activity is improved, especially in the co-oxidation reaction of cyclooctene and isobutyraldehyde, the cyclooctene conversion rate and the epoxy cyclooctene selectivity are improved, showing higher catalytic activity.
Smart Images

Figure CN116174019B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a composite catalytic material containing metal elements and molecular sieves, and a preparation method and application thereof. Background Art
[0002] In recent years, nanotechnology and the unique physical and chemical properties of nanoparticles have attracted widespread attention, and research involving "nano" in various fields has developed very rapidly. Through research, it is found that catalytic reactions often cannot occur on the bulk metal surface, and the catalytic problem is not a single molecule or single atom problem. The early concept believed that the active unit of catalysis is a collection of atomic clusters composed of several or more atoms. For example, the metal-supported catalysts used in petrochemicals have about 1018 active centers per cubic centimeter. When the specific surface area of the support is 50 to 300 m 2 ·g -1 Another important aspect is that among the catalyst supports currently used, molecular sieves with regular pore structures occupy a very important position. Depending on the raw material ratio and synthesis method, the effective pore size of this molecular sieve can be adjusted from a few tenths of nanometers to tens or even hundreds of nanometers. The catalytic reactions occurring in these nanopores with specific structures have very unique characteristics, such as location selectivity and molecular shape selectivity.
[0003] Due to the limitation of pores, microporous molecular sieves can only be diffused through by reactants of small molecular size, and thus cannot catalyze reactions involving macromolecular substrates. In view of this defect, mesopores or even macropores are introduced into microporous molecular sieves to construct molecular sieves with multi-level pore sizes, thereby improving the performance of microporous molecular sieves when applied to macromolecular reactants. According to different synthesis methods, the synthesis methods of multi-level pore molecular sieves mainly include the removal of skeleton atoms, the double template synthesis method of ordered micro-mesoporous composite molecular sieves, the hard template method, the dry gel conversion method and the silanization method. Among them, the silanization method is a relatively simple and widely used method. Since the silanol of the silanization agent hydrolyzes and condenses with the silanol of the molecular sieve precursor to produce a stable Si-O-Si bond, the effect of supporting layer pore expansion is ensured.
[0004] Wang Baorong et al. (CN111847471A) prepared a multi-level pore molecular sieve encapsulating active metals by introducing a silanization agent in the direct hydrothermal synthesis method. However, since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursor is very easy to form hydroxide precipitation. This problem has not been solved. The precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.), such as Wang et al. using ethylenediamine ligands and PdCl2 to form [Pd(NH2CH2CH2NH2)]Cl2 complex precursors, and then directly synthesized silicalite-1 molecular sieves (Pd@silicalite-1) with uniformly dispersed Pd nanoparticles embedded through hydrothermal crystallization. In summary, the metal precursor is complexed with an organic ligand and then introduced into the molecular sieve hydrothermal crystallization process, which is a more effective method for highly dispersed nanoparticles in molecular sieve crystals. The silanization method of introducing a silanization agent into the molecular sieve synthesis process is an effective and simple method for preparing a multi-level pore molecular sieve. However, it is difficult to achieve the above two purposes at the same time in general research in the prior art, and to obtain a molecular sieve with both advantages, that is, it is difficult to directly prepare a multi-level pore molecular sieve with highly dispersed metal nanoparticles. Summary of the invention
[0005] The purpose of the present disclosure is to provide a composite catalytic material containing metal elements and molecular sieves, and a preparation method and application thereof. The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have uniform particle size and are evenly dispersed in the molecular sieve pores.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal element M is a metal element capable of forming an oxide aggregate; the composite catalytic material has the following H2-TPR characteristics: the reduction peak temperature of the composite catalytic material in the H2-TPR test is T1, the reduction peak temperature of the oxide aggregate in the H2-TPR test is T2, T0 defined by the following formula (1) is any value between 350 and 600°C; T0=T1-T2 formula (1).
[0007] Optionally, the value of T0 is any value between 350 and 550°C.
[0008] Optionally, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve and silicon molecular sieves of other structures; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve; further preferably MFI structure molecular sieve;
[0009] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0010] Optionally, the metal M is Co, and the oxide aggregate is a Co3O4 aggregate;
[0011] The metal M is Mn, and the oxide aggregate is a MnO2 aggregate;
[0012] The metal M is Fe, and the oxide aggregate is Fe2O3 aggregate;
[0013] The metal M is Ni, and the oxide aggregate is NiO aggregate;
[0014] The metal M is Pd, and the oxide aggregate is a PdO aggregate;
[0015] The metal M is Pt, and the oxide aggregate is a PtO2 aggregate; or
[0016] The metal M is Cu, and the oxide aggregate is CuO aggregate.
[0017] Optionally, in the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.25):1, preferably (0.001-0.2):1.
[0018] Optionally, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.30-0.65mL / g, the micropore volume is 0.10-0.19mL / g, the mesopore volume is 0.18-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-8.0nm.
[0019] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a silanization agent and a peroxide to obtain a reaction mixture, wherein the silanization agent comprises at least one ligand complexed with the metal M ion; S2, performing a hydrothermal crystallization treatment and a calcination treatment on the reaction mixture.
[0020] Optionally, in step S1, the molar ratio of silicon source: template: water: metal element M: silanization agent calculated as SiO2 is 1: (0.001-1): (5-100): (0.001-0.25): (0.025-0.4), preferably 1: (0.005-0.5): (5-100): (0.001-0.2): (0.025-0.3); the molar ratio of peroxide to metal element M is (0.5-5): 1.
[0021] Optionally, step S1 includes:
[0022] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0023] b. adding peroxide to the aqueous solution of the metal M precursor, and mixing to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;
[0024] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;
[0025] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
[0026] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0027] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0028]
[0029] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R dEach is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0030] Optionally, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0031] R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from at least one of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group and a tert-butyl group;
[0032] Further preferably, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0033] The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0034] The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0035] Optionally, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0036] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0037] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0038] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0039] Preferably, the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0040] Optionally, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms;
[0041] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and -mercaptopropyltrimethoxysilane; further preferably, it is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0042] Optionally, in step S1, the peroxide is one or more of hydrogen peroxide or organic peroxides; the organic peroxide includes cumene hydroperoxide, ethylbenzene hydroperoxide and tert-butyl hydroperoxide.
[0043] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;
[0044] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0045] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0046] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0047] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The composite catalytic material is prepared by adding a metal precursor, a silanization agent and a peroxide to a crystallization system at the same time. The molecular sieve of the composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the molecular sieve of the prepared composite catalytic material has a multi-level pore structure, and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; in the H2-TPR test, the reduction peak temperature of the composite catalytic material is 350 to 600°C higher than the reduction peak temperature of the oxide aggregates of the metal element M, and the composite catalytic material has a high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0048] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0050] Figure 1 This is the H2-TPR spectrum of the metal-containing multi-level pore MFI structure molecular sieve prepared in Example 1. DETAILED DESCRIPTION
[0051] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0052] The inventors of the present disclosure surprisingly found in experiments that by introducing a metal precursor during the crystallization synthesis process of the molecular sieve, and then continuously introducing a silanization agent and a peroxide, and subjecting the obtained mixture to hydrothermal crystallization, washing and calcination, the obtained composite catalytic material including all-silicon molecular sieve and metal M oxide nanoparticles not only has a large specific surface area and pore volume performance, but also has uniform particle size of the metal oxide nanoparticles and is evenly dispersed in the molecular sieve pores. Moreover, when the value of T0 (i.e., T1-T2) in the composite catalytic material is above 350°C (T1 represents the reduction peak temperature of the composite catalytic material in the H2-TPR test, and T2 represents the reduction peak temperature of the oxide aggregates in the H2-TPR test), the composite catalytic material has good catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins. For example, when used for the co-oxidation reaction of cyclooctene and isobutyraldehyde, a higher cyclooctene conversion rate and epoxycyclooctene selectivity can be obtained.
[0053] The first aspect of the present disclosure provides a metal oxide nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal element M is a metal element capable of forming oxide aggregates;
[0054] The composite catalytic material has the following H2-TPR characteristics:
[0055] The reduction peak temperature of the composite catalytic material in the H2-TPR test is T1,
[0056] The reduction peak temperature of the oxide aggregate in the H2-TPR test is T2,
[0057] T0 defined by the following formula (1) is any value between 350 and 600°C;
[0058] T0=T1-T2 formula (1).
[0059] The present invention provides a composite catalytic material of metal oxide nanoparticles and molecular sieves. The molecular sieve of the composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; and the composite catalytic material has high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0060] In the present disclosure, metal M oxide aggregates refer to conventional oxide types obtained by calcining metal M precursors (such as nitrates, chlorides, etc.) known in the art during the synthesis of molecular sieves, for example, the oxide aggregates of metal cobalt are Co3O4 and the oxide aggregates of metal copper are CuO.
[0061] In the present disclosure, the H2-TPR test refers to a hydrogen temperature-programmed reduction characterization method, in which the composite catalytic material is reduced during the temperature-programmed reduction process, and information on the interaction between metal oxides or between metal oxides and the support during the reduction of the supported metal catalyst can be provided. The H2-TPR test in the present disclosure is performed on an AutoChemII2920, and the test conditions include: 10 vol% H2-90 vol% Ar, 50 ml / min, 60-900°C reduction.
[0062] In a preferred embodiment, the value of T0 is any value between 350 and 550° C. When T0 of the composite catalyst material is within this range, it has higher catalytic activity, cyclooctene conversion rate and epoxycyclooctene selectivity.
[0063] In one embodiment, the all-silicon molecular sieve in the composite catalytic material is one or more of MFI structure molecular sieve (such as S-1), MEL structure molecular sieve (such as S-2), BEA structure molecular sieve (such as Beta), MWW structure molecular sieve (such as MCM-22), two-dimensional hexagonal structure molecular sieve (such as MCM-41, SBA-15), MOR structure molecular sieve (such as MOR), TUN structure molecular sieve (such as TUN) and silicon molecular sieves of other structures (such as ZSM-48, MCM-48); preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve, such as the silicon molecular sieve is one of S-1, S-2 and Beta; further preferably, it is an MFI structure molecular sieve, such as S-1.
[0064] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; preferably selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum and copper.
[0065] In an optional embodiment, the metal M is Co, and the oxide aggregate is a Co3O4 aggregate;
[0066] In an optional embodiment, the metal M is Mn, and the oxide aggregate is a MnO2 aggregate;
[0067] In an optional embodiment, the metal M is Fe, and the oxide aggregate is Fe2O3 aggregate;
[0068] In an optional embodiment, the metal M is Ni, and the oxide aggregate is NiO aggregate;
[0069] In an optional embodiment, the metal M is Pd, and the oxide aggregate is a PdO aggregate;
[0070] In an optional embodiment, the metal M is Pt, and the oxide aggregate is a PtO2 aggregate;
[0071] In an optional embodiment, the metal M is Cu, and the oxide aggregate is CuO aggregate.
[0072] In one embodiment, in the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.25):1, preferably (0.001-0.2):1.
[0073] In one embodiment, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, the average particle size of the metal nanoparticles is 0.5 to 8.0 nm, preferably 1 to 7.5 nm; the BET specific surface area is 400 to 800 m 2 / g, preferably 400 to 750 m 2 / g; total pore volume is 0.3~0.65m 2 / g, preferably 0.31 to 0.63 m 2 / g; micropore volume is 0.1-0.19mL / g, preferably 0.11-0.18mL / g; mesopore volume is 0.15-0.46mL / g, preferably 0.18-0.46mL / g. The composite catalytic material disclosed in the present invention also has a multi-level pore structure, which is conducive to catalyzing reaction substrates of different sizes, especially the catalytic reaction of macromolecular substrates.
[0074] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nano-oxide particles and molecular sieves, comprising the following steps:
[0075] S1, mixing a template, a silicon source, water, a metal M precursor, a silanization agent and a peroxide to obtain a reaction mixture, wherein the silanization agent comprises at least one coordination group complexed with the metal M ion;
[0076] S2. performing hydrothermal crystallization and calcination on the reaction mixture.
[0077] The present invention introduces metal precursors, silanization agents and peroxides into the molecular sieve synthesis raw materials, which can take into account the effects of highly dispersed metal oxide nanoparticles and molecular sieve support layer pore expansion, and prepare a multi-level porous molecular sieve composite catalytic material with highly dispersed metal oxide nanoparticles.
[0078] In the present disclosure, peroxide can play the role of complexing metals, so as to achieve the effect of dispersing and stabilizing metals; a silanization agent with one or more coordination groups (the coordination groups can be, for example, at least one of amine, thiol, and oxygen-containing coordination groups) is also added to the reaction mixture, and the coordination groups can also complex metals to achieve the effect of fixing and dispersing metals, and the supporting layer effect of the alkyl chain plays a pore expansion effect; thus, a multi-level pore all-silicon molecular sieve with highly dispersed metal metal oxide nanoparticles is prepared. In addition, the highly dispersed metal M oxide nanoparticles formed by the metal M introduced during the synthesis of the molecular sieve enter the molecular sieve crystals, and some metal oxide nanoparticles can also be formed between the crystals and on the surface (such as the pore surface) of the molecular sieve.
[0079] In one embodiment, the molar ratio of silicon source: template: water: metal element M: silanization agent in terms of SiO2 is 1: (0.001-1): (5-100): (0.001-0.25): (0.025-0.4), preferably 1: (0.005-0.5): (5-100): (0.001-0.2): (0.025-0.3); the molar ratio of peroxide to metal element M is (0.5-5): 1. Specifically, the water used in step S1 can be water commonly used in the synthesis of molecular sieves, and in order to avoid the introduction of heteroatoms, it is preferably deionized water.
[0080] In a preferred embodiment, step S1 comprises:
[0081] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0082] b. adding peroxide to the aqueous solution of the metal M precursor, and mixing to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;
[0083] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0084] In one embodiment, in step S1, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black; the general formula of the organic silicone grease is the structure shown in the following formula (A):
[0085]
[0086] Where R a , R b , R c , R dEach is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight chain alkyl group having 1 to 4 carbon atoms or a branched chain alkyl group having 3 to 4 carbon atoms. a , R b , R c , R d Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl. a , R b , R c , R d Each is independently methyl or ethyl.
[0087] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0088] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.
[0089] Further preferably, the template is selected from at least one of the quaternary ammonium bases having the following general formula (B):
[0090] R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from at least one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0091] The template agent is preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide (including various isomers of tetrapropylammonium hydroxide, such as tetra-n-propylammonium hydroxide and tetraisopropylammonium hydroxide) and tetrabutylammonium hydroxide (including various isomers of tetrabutylammonium hydroxide, such as tetra-n-butylammonium hydroxide and tetraisobutylammonium hydroxide).
[0092] In a preferred embodiment, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0093] The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0094] The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide. The present disclosure can prepare molecular sieves with different structures by selecting different template agents.
[0095] In one embodiment, in step S1, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0096] The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95°C for 2-10 hours; preferably stirring and hydrolyzing at 50-95°C for 2-8 hours. Preferably, the hydrolysis and alcohol removal treatment makes the mass content of alcohol produced by hydrolysis of the obtained organic silicone grease in the hydrolyzed silicon solution less than 10 ppm.
[0097] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal (such as a compound containing a metal element and / or a metal single substance) can achieve the purpose of the present disclosure.
[0098] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the organic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0099] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0100] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0101] In one embodiment, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, preferably 1 to 12; the number of carbon atoms of the aromatic group can be 6 to 18, preferably 6 to 12;
[0102] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0103] In one embodiment, in step S1, the peroxide is one or more of hydrogen peroxide or organic peroxides; the organic peroxides include cumene hydroperoxide (CHP), ethylbenzene hydroperoxide (EBHP) and tert-butyl hydroperoxide (TBHP).
[0104] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.
[0105] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.
[0106] The third aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves prepared according to the method described in the second aspect of the present disclosure.
[0107] The fourth aspect of the present disclosure provides the use of the metal oxide nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0108] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite catalytic material is 1 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.
[0109] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.
[0110] The present disclosure will be further described below using embodiments.
[0111] In the present disclosure, H2-TPR experiment was carried out on AutoChemII2920, and the experimental conditions were: 10% H2-90% Ar, 50 ml / min, 60-900°C reduction.
[0112] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.
[0113] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0114] In the present disclosure, the X-ray diffraction (XRD) crystal phase diagram of the sample is measured on a Siemens D5005 X-ray diffractometer, the radiation source is Kα (Cu), and the test range 2θ is 0.5° to 70°.
[0115] The cobalt nitrate used in the embodiments of the present disclosure is all cobalt nitrate hexahydrate.
[0116] Example 1
[0117] (1) 1.6 g of a 25.05 wt % tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol) and 52.8 g (3 mol) of water were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;
[0118] (2) 0.03 g of cobalt nitrate hexahydrate (0.0001 mol) and 0.18 g (0.01 mol) of water were stirred evenly, and then 0.05 mmol of H2O2 was added, and the aqueous solution of cobalt was mixed with the hydrolyzed solution of silicon obtained in step (1);
[0119] (3) adding 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) to the mixture of step (2) and stirring for 0.5 hour;
[0120] (4) The mixture obtained in step (3) was transferred to a stainless steel sealed reactor and crystallized at 175°C for 24 hours to obtain a sample. The obtained sample was filtered, washed, dried at 110°C for 6 hours, and then calcined in a muffle furnace at 600°C for 6 hours to obtain a composite catalytic material product of metal oxide nanoparticles and multi-level pore all-silicon molecular sieve, which was denoted as C-1. Its H2-TPR graph is shown in FIG. Figure 1 shown.
[0121] The BET specific surface area, total pore volume, micropore volume, mesopore volume and the average particle size of the metal nanoparticles contained in C-1 are listed in Table 2. The H2-TPR spectrum of C-1 is shown in Figure 1 shown.
[0122] Comparative Example 1
[0123] This comparative example was prepared according to the method of Example 1, except that no silanization agent was added. The ratio, synthesis conditions and results are listed in Table 1. Other conditions and operations were the same as those of Example 1. The prepared product was recorded as sample DC-1.
[0124] Comparative Example 2
[0125] Under stirring conditions, ethyl orthosilicate, tetrapropylammonium hydroxide, cobalt nitrate and deionized water are mixed to obtain a first mixture with a molar ratio of SiO2: structure directing agent: Co: H2O = 1:0.2:0.001:30; stirring at 50° C. for 2 hours;
[0126] Then, PHAPTMS was added to the first mixture at a molar ratio of SiO2: silanization agent = 1: 0.025, and stirred for 0.5 hours. The obtained second mixture was transferred to a pressure-resistant stainless steel reactor; heated to 170°C and crystallized under autogenous pressure for 8 hours under stirring conditions. After the stainless steel pressure-resistant reactor was cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous molecular sieve encapsulating molybdenum. The prepared product was recorded as sample DC-2.
[0127] Comparative Example 3
[0128] This comparative example was prepared according to the method of NingWang et al. (JACS, 2016, Vol. 138, pp. 7484-7487).
[0129] First, deionized water was mixed with 10.8g TPAOH solution and stirred continuously for 10 minutes, and then 8.32g ethyl orthosilicate (0.04mol) was added. After continuous stirring for 6 hours, the mixture became clear after complete hydrolysis. 0.012g cobalt nitrate hexahydrate (0.041mmol, the molar ratio of metal cobalt to silicon source was 0.001) was dissolved in a mixture of 0.3mL ethylenediamine and 3mL water to prepare [Pd(NH2CH2CH2NH2)2]Cl2 solution, and then the resulting solution was added dropwise to the above mixture and stirred for 30min without precipitation. The reaction mixture was transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner and static crystallization was performed at 170°C in a conventional oven for 4 days. The solid product was centrifuged, washed with water and ethanol several times, dried in an oven at 80°C overnight, roasted in an air atmosphere at 550°C for 8 hours, and finally reduced with hydrogen to obtain the product. The prepared product was recorded as sample DC-3.
[0130] Embodiment 2 to Embodiment 9
[0131] The corresponding products C-2 to C-9 were prepared according to the method of Example 1, and their proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations are similar to those of Example 1.
[0132] Example 10
[0133] The metal-containing multi-level porous β molecular sieve was prepared by referring to the method of Example 1, but the ratio and template agent were changed. The template agent used was tetraethylammonium hydroxide (TEAOH). The ratio, synthesis conditions and results are shown in Table 1. The prepared product was recorded as sample C-10.
[0134] Embodiment 11
[0135] The cobalt-containing multi-level porous MEL molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent, and using tetrabutylammonium hydroxide (TBAOH) as the template agent. The ratio, synthesis conditions and results are shown in Table 1. The prepared product is recorded as sample C-11.
[0136] Example 12
[0137] The cobalt-containing multi-level porous MFI molecular sieve was prepared by referring to the method of Example 1, and the proportions, synthesis conditions and results are shown in Table 1. The hydrothermal crystallization temperature was 130°C and the hydrothermal crystallization time was 6 days; the calcination temperature was 850°C and the calcination time was 9 hours. The prepared product was recorded as sample C-12.
[0138] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of the metal nanoparticles contained in the products obtained in the above examples and comparative examples are listed in Table 2 below.
[0139] Table 1
[0140]
[0141]
[0142] In Table 1, TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane); CHP is cumene hydroperoxide, and TBHP is tert-butyl hydroperoxide. The reagents used in the present disclosure can be obtained through conventional purchasing channels.
[0143] Table 2
[0144]
[0145] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0146] According to Table 2, compared with DC-1 prepared in Comparative Example 1 (without adding silanizing agent and peroxide) and DC-3 prepared in Comparative Example 3 (without adding silanizing agent and peroxide), C-1 to C-12 prepared in Examples 1 to 12 of the present disclosure have products with higher mesopore volume after adding silanizing agent and peroxide during the preparation process, indicating that the method provided in the present disclosure can effectively expand the pores of the molecular sieve.
[0147] Compared with DC-1 to DC-3, C-1 to C-12 provided in the embodiments of the present disclosure can simultaneously have higher BET specific surface area, total pore volume, mesopore volume, and smaller average particle size of nanoparticles, indicating that the metal nanoparticles in the composite catalytic material provided by the present disclosure have a lower degree of aggregation and better dispersion.
[0148] Test Case
[0149] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0150] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.
[0151] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):
[0152]
[0153]
[0154]
[0155] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1 MPa, the amount of cyclooctene was 1 mmol, the amount of catalyst was 50 mg, and the amount of solvent acetonitrile was 2.5 mL. The reaction was stable at 25°C for 6 hours, and samples were taken for analysis. The results are shown in Table 3.
[0156] Table 3
[0157]
[0158]
[0159] In the embodiment, the T2 value of the oxide aggregate Co3O4 of the metal element cobalt is 350°C; the T2 value of the oxide aggregate NiO of the metal element nickel is 450°C; the T2 value of the oxide aggregate MnO2 of the metal element manganese is 300°C; the T2 value of the oxide aggregate Fe2O3 of the metal element iron is 560°C; and the T2 value of the oxide aggregate ZnO of the metal element zinc is 390°C.
[0160] According to the data in Table 3, compared with DC-1 to DC-3, the metal oxide nanoparticles and molecular sieve composite catalytic materials C-1 to C-12 prepared in Examples 1 to 12 of the present disclosure have a T0 of 350 to 600°C, and have higher catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde, and have higher cyclooctene conversion rate and epoxycyclooctene selectivity.
[0161] Furthermore, by comparing C-1 to C-11 with C-12, it can be seen that the T0 value of C-1 to C-11 is any value between 350°C and 550°C, and the composite catalytic materials C-1 to C-11 have higher catalytic activity, cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity.
[0162] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0163] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0164] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A composite catalytic material of metal nanoparticles and molecular sieves, It is characterized in that It comprises an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal element M is a metal element capable of forming oxide aggregates; the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; The composite catalytic material has the following H 2 -TPR Features: The composite catalytic material is 2 -The reduction peak temperature in the TPR test is T 1 , The oxide aggregates in H 2 -The reduction peak temperature in the TPR test is T 2 , T is defined as follows: 0 Any value between 350~600℃; T 0 = T 1 -T 2 Formula (1); The composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a silanization agent and a peroxide to obtain a reaction mixture, wherein the silanization agent comprises at least one coordination group complexed with the metal M ion; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments; The general formula of the silanization agent is R 5 Si(R 6 )(R 7 )R 8 , where R 5 , R 6 , R 7 , R 8 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R 5 , R 6 , R 7 , R 8 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the alkyl group, the alkoxy group, the thiol group and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms; The peroxide is one or more of hydrogen peroxide or organic peroxide; the organic peroxide includes cumene hydroperoxide, ethylbenzene hydroperoxide and tert-butyl hydroperoxide.
2. The composite catalytic material according to claim 1, It is characterized in that The T 0 The value is any value between 350~550℃.
3. The composite catalytic material according to claim 1, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve, TUN structure molecular sieve and silicon molecular sieves of other structures.
4. The composite catalytic material according to claim 3, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the group consisting of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
5. The composite catalytic material according to claim 4, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, the MEL structure molecular sieve and the BEA structure molecular sieve.
6. The composite catalytic material according to claim 5, It is characterized in that The all-silicon molecular sieve in the composite catalytic material is an MFI structure molecular sieve.
7. The composite catalytic material according to claim 1, It is characterized in that The metal M is Co, and the oxide aggregate is Co 3 O 4 Aggregates; The metal M is Mn, and the oxide aggregate is MnO 2 Aggregates; The metal M is Fe, and the oxide aggregate is Fe 2 O 3 Aggregates; The metal M is Ni, and the oxide aggregate is NiO aggregate; The metal M is Pd, and the oxide aggregate is a PdO aggregate; The metal M is Pt, and the oxide aggregate is PtO 2 Aggregates; or The metal M is Cu, and the oxide aggregate is CuO aggregate.
8. The composite catalytic material according to claim 1, It is characterized in that In the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.25):
1.
9. The composite catalytic material according to claim 8, It is characterized in that In the composite catalytic material, the molar ratio of the metal M element to the silicon element is (0.001-0.2):
1.
10. The composite catalytic material according to claim 1, It is characterized in that The BET specific surface area of the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.30~0.65mL / g, the micropore volume is 0.10~0.19mL / g, the mesopore volume is 0.15~0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~8.0nm.
11. The composite catalytic material according to claim 1, It is characterized in that In step S1, SiO 2 The molar ratio of silicon source: template: water: metal element M: silanization agent is 1: (0.001~1): (5~100): (0.001~0.25): (0.025~0.4); the molar ratio of peroxide to metal element M is (0.5~5):
1.
12. The composite catalytic material according to claim 11, It is characterized in that In step S1, SiO 2 The molar ratio of silicon source: template: water: metal element M: silanization agent is 1: (0.005~0.5): (5~100): (0.001~0.2): (0.025~0.3).
13. The composite catalytic material according to claim 1, It is characterized in that Step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. adding peroxide to the aqueous solution of the metal M precursor, and mixing to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material; c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
14. The composite catalytic material according to claim 1, It is characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
15. The composite catalytic material according to claim 14, It is characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
16. The composite catalytic material according to claim 15, It is characterized in that The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
17. The composite catalytic material according to claim 16, It is characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
18. The composite catalytic material according to claim 17, It is characterized in that The R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
19. The composite catalytic material according to claim 18, It is characterized in that The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
20. The composite catalytic material according to claim 1, It is characterized in that In step S1, the template agent is an organic base.
21. The composite catalytic material according to claim 20, It is characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
22. The composite catalytic material according to claim 21, It is characterized in that The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); R 1 , R 2 , R 3 and R 4 are independently selected from alkyl groups having 1 to 4 carbon atoms.
23. The composite catalytic material according to claim 22, It is characterized in that In formula (B), R 1 , R 2 , R 3 and R 4 are independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms.
24. The composite catalytic material according to claim 23, It is characterized in that In formula (B), R 1 , R 2 , R 3 and R 4 Each of the at least one groups is selected from the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
25. The composite catalytic material according to claim 1, It is characterized in that The molecular sieve in the composite catalyst material is an MFI molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
26. The composite catalytic material according to claim 13, It is characterized in that In step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain a hydrolyzed solution of the silicon; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
27. The composite catalytic material according to claim 26, It is characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
28. The composite catalytic material according to claim 1, It is characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M.
29. The composite catalytic material according to claim 28, It is characterized in that The metal M precursor is a water-soluble inorganic salt of metal M.
30. The composite catalytic material according to claim 13, It is characterized in that The molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
31. The composite catalytic material according to claim 1, It is characterized in that In step S1, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and -mercaptopropyltrimethoxysilane.
32. The composite catalytic material according to claim 31, It is characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
33. The composite catalytic material according to claim 1, It is characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
34. The composite catalytic material according to claim 33, It is characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.
35. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 34 in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins.
36. The use according to claim 35, It is characterized in that The use includes use of the metal nanoparticles and molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
Citation Information
Patent Citations
Hierarchical pore titanium silicalite molecular sieve for packaging active metal and preparation method thereof
CN111847471A
High-dispersion dual-functional catalyst for hydrogenating and deoxidizing phenol and preparation method of catalyst
CN102698788A
All-silicon molecular sieve and synthetic method thereof
CN104556087A