A method for preparing porous molecular sieve using unroasted rice husk as template

Porous molecular sieves are prepared by crushing unroasted rice husk and high-temperature hydrothermal reaction, which solves the problems of complex process and high energy consumption, and realizes the preparation of environmentally friendly and low-cost molecular sieves with excellent texture properties and wide application prospects.

CN116177562BActive Publication Date: 2024-10-29HUAQIAO UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211547995.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-10-29
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

In the existing technology, the process for preparing porous molecular sieves from rice husks is complex and requires roasting, which results in high energy consumption and is not environmentally friendly, and the preparation cost of traditional silica is high.

Method used

Using unroasted rice husk as a template, porous molecular sieves are prepared through crushing and high-temperature hydrothermal reaction to simplify the process and reduce energy consumption. The particle size and pore structure of the molecular sieve are controlled by regulating the crushing mesh number and adding amount of rice husk.

Benefits of technology

The process is simplified, energy-saving and environmentally friendly, and the cost of molecular sieve synthesis is reduced. The prepared molecular sieve has superior texture properties and is suitable for catalysis and environmental fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116177562B_ABST
    Figure CN116177562B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a porous molecular sieve using unbaked rice husk as a template, comprising the following steps: step (1), pre-treating the rice husk, crushing, and sieving; step (2), subjecting water, a template agent, an aluminum source, and rice husk powder to a high-temperature hydrothermal reaction; step (3), washing, drying, and roasting the product after the hydrothermal reaction; step (1), comprising the following steps: a pre-treatment step, comprising soaking and washing with clean water to remove dust from the rice husk; crushing the rice husk with a pulverizer, and sieving rice husk powder with a specific mesh range with sieves of different meshes. The present invention uses unbaked rice husk as a biological template, and can flexibly regulate the particle size and pore structure of the molecular sieve through a simple physical crushing process; by adjusting the mesh number of the rice husk and controlling the amount of the rice husk, the silicon element in the rice husk can be promoted to participate in the synthesis system of the molecular sieve, which can solve the problem of high molecular sieve synthesis cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a porous molecular sieve by taking unroasted rice husk as a template, and belongs to the field of waste biomass resource utilization. Background Art

[0002] Problems such as the greenhouse effect caused by excessive emissions of carbon dioxide (CO2) have seriously threatened the survival of humans and other creatures on Earth. Therefore, how to solve the emission of CO2 has attracted much attention. Among them, the arbitrary disposal of agricultural waste (such as direct burning of straw) has attracted widespread attention. Rice is the most important food crop in Asia. The amount of rice husks produced by my country's annual rice cultivation accounts for about 30% of the world's total production, ranking first in the world. According to the national grain production data for 2021 released by the National Bureau of Statistics, the annual output of rice is as high as 212.84 million tons, of which rice husks account for about 20wt% of the total mass of rice, equivalent to an output of about 42.56 million tons.

[0003] The preparation of traditional silicon dioxide usually requires the use of silicon alkoxides and silicates as silicon sources, and the cost of raw materials is extremely high. Therefore, it is particularly important to seek a low-cost method for preparing silicon dioxide. Rice husk is a natural composite material with inorganic silicon dioxide and organic fibers (cellulose, hemicellulose, lignin) as the main components. After investigation, the silicon content of the product after roasting rice husk is as high as more than 90wt%, which has the potential to be used as a biomass silicon source.

[0004] For example, in application publication number CN 111892065 A. A Chinese invention patent application entitled “A method for preparing SAPO-34 molecular sieve using rice husk as silicon source” discloses a method for preparing SAPO-34 molecular sieve using rice husk as silicon source, and the specific steps are as follows: (1) pretreatment: wash and dry the rice husk, and place it in a muffle furnace for pyrolysis to obtain rice husk ash; (2) mixed pre-crystallization: use rice husk ash as silicon source and hard template agent, use deionized water as solvent, mix aluminum source, phosphorus source, rice husk ash, template agent, deionized water and SAPO-34 molecular sieve raw powder in proportion, and stir for a certain time; (3) crystallization: place the mixture obtained in step (2) in a polytetrafluoroethylene reactor for hydrothermal reaction. After the reaction is completed, take out the product, centrifuge, wash, and filter, and dry the filter cake to obtain SAPO-34 molecular sieve coarse powder; (4) post-treatment: calcine the SAPO-34 molecular sieve coarse powder at high temperature in a muffle furnace to remove the template agent and obtain pure SAPO-34 molecular sieve powder. In this patent, rice husk pretreatment requires pyrolysis at 400-800°C in a muffle furnace for 3-4 hours to obtain rice husk ash, which consumes a lot of energy and is not environmentally friendly.

[0005] In the application publication number CN 105731485 A, entitled “A method for preparing multi-level pore zeolite molecular sieve using rice husk”, a method for preparing multi-level pore zeolite molecular sieve using rice husk is disclosed. In the method, the rice husk is pretreated, specifically, 300-500g of rice husk is taken, 40-50℃ clean water is added thereto, stirred and washed for 20-30min to remove surface impurities, filtered, the filter residue is placed in an oven for drying, crushed after drying, passed through a 40-50 mesh sieve, 30-50g of the sieved rice husk is taken and placed in a round-bottom flask, 200-300mL of 2-4% hydrochloric acid is added to the flask for mixing, and 10 Reflux in an oil bath at 5 to 115 ° C for 1 to 2 hours, cool to room temperature after reflux, filter, obtain filter residue, and dry; add the dried rice husk to the titanium dioxide sol at a solid-liquid ratio of 1: 8 to 1: 10, stir and put it into an ultrasonic dispersion instrument for dispersion for 20 to 30 minutes, let it stand for 2 to 3 hours after uniform dispersion, load it into a blast oven and dry it at 105 to 115 ° C, add the dried material to a crucible, place it in a muffle furnace for treatment, and heat it from 25 ° C to 1200 ° C under nitrogen protection, with a heating rate of 12 ° C / min, treat it for 1 to 2 hours, cool it to room temperature after treatment and then take it out. The rice husk pretreatment process of the above patent is complicated, and the rice husk needs to be roasted before preparing the molecular sieve.

[0006] In view of this, the inventor of this case conducted in-depth research on the above-mentioned issues, which led to the emergence of this case. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a porous molecular sieve using unroasted rice husk as a template, which is simple in process, more energy-saving and environmentally friendly

[0008] In order to achieve the above object, the present invention adopts such technical solution:

[0009] A method for preparing a porous molecular sieve using unroasted rice husk as a template comprises the following steps:

[0010] Step (1), pre-treating, crushing and sieving rice husks;

[0011] Step (2), subjecting water, a template, an aluminum source and rice husk powder to a high-temperature hydrothermal reaction;

[0012] Step (3), washing, drying and calcining the product after the hydrothermal reaction;

[0013] Step (1) includes the following steps:

[0014] (a) a pretreatment step, comprising soaking and washing with clean water to remove dust from the rice husk, and then drying for later use;

[0015] (b) crushing rice husks by a crusher, and sieving rice husk powder with a specific mesh size range using sieves with different mesh sizes;

[0016] Step (2) includes the following steps:

[0017] (a) the rice husk powder obtained in step (1) is fully mixed with water, a template agent and an aluminum source and then placed in an oven for heating;

[0018] (b) placing the sample treated in step (a) into a hydrothermal reactor for high-temperature hydrothermal reaction;

[0019] Step (3) includes the following steps:

[0020] (a) washing the sample obtained in step (2) and separating the product by high-speed centrifugation;

[0021] (b) The product is placed in an oven to dry at a constant temperature, and then placed in a muffle furnace for calcination to remove the template and organic components.

[0022] As a preferred embodiment of the present invention, the water soaking time of step (a) in step (1) is 2-24 hours, and the drying temperature is 20-150°C.

[0023] As a preferred embodiment of the present invention, the rice husk powder in step (b) of step (1) has a mesh size of 20-300 meshes.

[0024] As a preferred embodiment of the present invention, the template agent in step (a) in step (2) is tetrapropylammonium hydroxide; the aluminum source is sodium aluminate, and the components in step (a) in step (2) are added in the following proportions: 1-20 mL of water, 1-6 g of rice husks, 1-15 mL of tetrapropylammonium hydroxide, and 0.01-0.1 g of sodium aluminate.

[0025] As a preferred embodiment of the present invention, in step (2), the heating temperature of the oven in step (a) is 60-160° C., and the heating time is 1-12 h.

[0026] As a preferred embodiment of the present invention, the high temperature hydrothermal treatment temperature of step (b) in step (2) is 80-240° C. and the time is 6-24 hours.

[0027] As a preferred embodiment of the present invention, the cleaning agent used in step (a) of step (3) is water or ethanol.

[0028] As a preferred embodiment of the present invention, in step (b) of step (3), the temperature of the constant temperature drying oven is 20-150°C, the calcination temperature of the muffle furnace is 200-800°C, the calcination time is 2-12h, and the heating rate ranges from 2-20°C / min.

[0029] As a preferred embodiment of the present invention, in step (2), the rice husk powder, water, template, aluminum source and silicon source are fully mixed and then placed in an oven for heating, and the silicon source is tetraethyl orthosilicate, and the amount added is greater than 0 mL and less than 15 mL. As a preferred embodiment of the present invention, the mesh size of the rice husk powder in step (b) of step (1) is 20-300 mesh.

[0030] After adopting the technical scheme of the present invention, unroasted rice husks are used as biological templates, and the particle size and pore structure of the molecular sieve can be flexibly adjusted through simple physical crushing treatment; by adjusting the mesh size of the rice husks and controlling the amount of the added rice husks, the silicon element in the rice husks can be promoted to participate in the synthesis system of the molecular sieve, and even no external silicon source is required, which can solve the problem of high molecular sieve synthesis cost; due to the multi-level spatial structure of the rice husks, the molecular sieve prepared by the present invention has more superior texture performance, can effectively adjust the pore structure of the molecular sieve, and the method has good repeatability and has broad application prospects in the fields of catalysis and environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The crystal forms of the effects of different mesh sizes and addition amounts of rice husks on the particle size of the molecular sieve obtained in Examples 1-6 of the present invention are characterized by using an X-ray powder diffractometer produced by Rigaku, model SmartLab, which is equipped with a Cu Kα radiation source (λ=1.54182) of 40 kV and 30 mA, and a detection range of 5-70°;

[0032] Figure 2 The electron microscope pictures of the effects of different mesh sizes on the particle size of the molecular sieve obtained in Examples 1-6 of the present invention are shown. The scanning electron microscope characterization test instrument is produced by Hitachi, model S-4800. DETAILED DESCRIPTION

[0033] In order to further explain the technical solution of the present invention, it is described in detail below in conjunction with embodiments.

[0034] Example 1

[0035] A method for preparing a porous molecular sieve with adjustable particle size using unroasted rice husk as a template comprises the following steps:

[0036] Step (1) includes the following steps:

[0037] (a) soaking the rice husks obtained from the factory in clean water for 4 hours to remove the dust from the rice husks, and then drying them at 80°C;

[0038] (b) crushing rice husks with a crusher to obtain rice husk powder with a mesh size of 20-60;

[0039] Step (2) includes the following steps:

[0040] (a) 1.5 g of the rice husk powder dried in step (b) of step (1) was taken, and 5 mL of water was added; 7.2 mL of a 25 wt% aqueous solution of tetrapropylammonium hydroxide; 0.097 g of sodium aluminate powder; and 8 mL of tetraethyl orthosilicate were added. After being stirred for 3 h, the mixture was heated in an oven at 80° C. for 2 h.

[0041] (b) The sample in the oven is cooled to room temperature and then placed in a high-pressure sealed reactor.

[0042] The hydrothermal reaction was carried out at 170 °C for 12 h;

[0043] Step (3) includes the following steps:

[0044] (a) washing the sample obtained in step (2) with clean water, and separating the product by centrifuge;

[0045] (b) The product was dried in an oven at 80°C for two hours and then calcined in a muffle furnace (setting parameters: 550°C, 5h, heating rate 5°C / min).

[0046] Referring to the process parameters of the present invention, rice husk is used as a biological template to participate in the synthesis of molecular sieve. Figure 2 As shown in a and b, the sample is magnified by scanning electron microscopy and it can be seen that the molecular sieve grows along the rice husk template. The molecular sieve particle size is at the nanometer level (the average particle size is about 126nm). The molecular sieve is like a short cylindrical strip, and its appearance replicates the multi-level and multi-dimensional spatial structure of the rice husk, with rich pore structure (such as Figure 2 a, b). XRD spectrum characterization proves that the product of Example 1 is ZSM-5 zeolite ( Figure 1 ).

[0047] Example 2

[0048] In step a of step (2) of Example 1, rice husks are crushed and sieved to 60-100 mesh before being added, and the remaining process parameters are the same as those of Example 1. Figure 2 As shown in c and d, the sample is magnified by a scanning electron microscope and it can be seen that the molecular sieve grows along the rice husk template platform, and the molecular sieve particle size suddenly increases near the platform, like a "coral reef" with molecular sieves growing on it. The rice husk surface has protrusions but the outline is not very clear, and smaller molecular sieves are distributed around it. The molecular sieve particle size scale is nanometer level (average particle size is about 200nm), and the molecular sieve particles are like cylindrical short strips. Its appearance replicates the multi-level and multi-dimensional spatial structure of rice husks. Characterization by XRD spectra proves that the product of Example 2 is ZSM-5 zeolite (such as Figure 1 ).

[0049] Example 3

[0050] In step a of step (2) of Example 1, rice husks are crushed and sieved to 100-200 mesh before being added, and the remaining process parameters are the same as those of Example 1. Figure 2 As shown in Figures e and f, the sample was magnified by a scanning electron microscope, and it was found that the molecular sieve grew along the rice husk template platform, the particle outlines of the protruding surface became clear, and the smaller molecular sieves were distributed around. The molecular sieve particle size was nanometer level (average particle size was about 220nm), and the molecular sieve particles were cylindrical and short strip-shaped, and their appearance replicated the multi-level and multi-dimensional spatial structure of the rice husk. The XRD spectrum characterization proved that the product of Example 3 was ZSM-5 zeolite (such as Figure 1 ).

[0051] Example 4

[0052] In step a of step (2) of Example 1, the rice husk is crushed and sieved to obtain 100-200 mesh, and the added amount is adjusted to 3g, and the other process parameters are the same as those of Example 1. Figure 2 As shown in g and h, the sample was magnified by a scanning electron microscope and it was found that the molecular sieve grew along the rice husk template platform. At this time, the platform was not very obvious, and the particle size suddenly increased. The molecular sieve with uniform morphology and particle size was observed, and its particle size scale was nanometer level (average particle size was about 350nm). The molecular sieve particles were cylindrical and short strip-shaped, and their appearance was similar to the multi-level and multi-dimensional spatial structure of rice husk, indicating that the molecular sieve successfully replicated the morphology of rice husk. The XRD spectrum was characterized to prove that the product of Example 4 was ZSM-5 zeolite (such as Figure 1 ).

[0053] Example 5

[0054] In step a of step (2) of Example 1, the rice husk is crushed and then sieved to obtain 100-200 mesh, and the added amount is adjusted to 6g, and the other process parameters are the same as those of Example 1. Figure 2 As shown in Figs. i and j, the sample was magnified by a scanning electron microscope and it was found that the molecular sieve "grew" from the surface of the rice husk template platform in the form of a long flat plate. The surface of the rice husk was covered with molecular sieve (average particle size of about 2.89 um) and maintained a good morphology of the rice husk. The XRD spectrum characterization proved that the product of Example 5 was ZSM-5 zeolite (such as Figure 1 ).

[0055] Example 6

[0056] In step a of step (2) of Example 1, the rice husks are crushed and then sieved to obtain 100-200 mesh, and the added amount is adjusted to 6g, and tetraethyl orthosilicate is not added. The other process parameters are the same as those of Example 1. Figure 2As shown in k and l, the biomaterial is magnified by scanning electron microscopy and it can be seen that the micron-level molecular sieve is distributed on the surface of the rice husk template. The molecular sieve is elliptical (with an average particle size of about 3.95um), indicating that the silicon source of the molecular sieve synthesis is all from the rice husk template, and it can still maintain the multi-level and multi-dimensional spatial structure morphology of the rice husk (such as Figure 1 The XRD spectrum characterization proves that the product of Example 6 is ZSM-5 zeolite with good crystallinity (such as Figure 1 ).

[0057] The present invention can synthesize porous molecular sieves with different particle sizes by only adding rice husk powder crushed into different mesh sizes into the synthesis reaction system of molecular sieve; when the rice husk mesh size is fixed, the amount of rice husk added is adjusted, and the bio-templated molecular sieve shows different particle size scales and morphologies, and the unbaked rice husk can replace the use of conventional silicon sources in the process of synthesizing molecular sieves. The method can regulate the morphology and particle size of molecular sieve synthesis, has low production cost, and is conducive to the comprehensive utilization of waste rice husk resources.

[0058] The product form of the present invention is not limited to the embodiments of this case. Any appropriate changes or modifications made by anyone with similar ideas should be deemed to be within the patent scope of the present invention.

Claims

1. A method for preparing a porous molecular sieve using unroasted rice husk as a template, Features: The following steps are involved: Step (1), pre-treating, crushing and sieving rice husks; Step (2), subjecting water, template, aluminum source and rice husk powder to a high temperature hydrothermal reaction; Step (3), washing, drying and calcining the product after the hydrothermal reaction; Step (1) includes the following steps: (a) a pretreatment step, comprising soaking and washing with clean water to remove dust from the rice husk, and then drying for later use; (b) crushing the rice husks by a crusher, and sieving the rice husk powder with a mesh size range of 20-300 meshes or 20-100 meshes by using sieves with different mesh sizes; Step (2) includes the following steps: (a) The rice husk powder obtained in step (1) is fully mixed with water, a template agent, and an aluminum source, and then placed in an oven for heating; the template agent is tetrapropylammonium hydroxide; the aluminum source is sodium aluminate, and the components are added in the following proportions: 1-20 mL of water, 1-6 g of rice husk, 1-15 mL of tetrapropylammonium hydroxide, and 0.01-0.1 g of sodium aluminate powder; (b) placing the sample treated in step (a) into a hydrothermal reactor for high-temperature hydrothermal reaction; Step (3) includes the following steps: (a) washing the sample obtained in step (2) and separating the product by high-speed centrifugation; (b) The product is placed in an oven to dry at a constant temperature, and then placed in a muffle furnace for calcination to remove the template and organic components.

2. A method for preparing a porous molecular sieve using unroasted rice husk as a template as claimed in claim 1, Features: The soaking time of step (a) in the step (1) is 2-24 h, and the drying temperature is 20-150°C.

3. A method for preparing a porous molecular sieve using unroasted rice husk as a template as claimed in claim 1, Features: In the step (2), the oven heating temperature in step (a) is 60-160° C., and the heating time is 1-12 h.

4. A method for preparing a porous molecular sieve using unroasted rice husk as a template as claimed in claim 3, Features: The high temperature hydrothermal treatment temperature of step (b) in step (2) is 80-240° C. and the time is 6-24 h.

5. A method for preparing a porous molecular sieve using unroasted rice husk as a template as claimed in claim 4, Features: The cleaning agent used in step (a) of step (3) is water or ethanol.

6. A method for preparing a porous molecular sieve using unroasted rice husk as a template as claimed in claim 5, Features: In step (b) of step (3), the temperature of the constant temperature drying oven is 20-150°C, the temperature of the muffle furnace is 200-800°C, the time is 2-12 h, and the heating rate ranges from 2-20°C / min.

7. A method for preparing a porous molecular sieve using unroasted rice husk as a template as claimed in claim 6, Features: In step (2), in step (a), the rice husk powder is fully mixed with water, a template, an aluminum source, and a silicon source, and then placed in an oven for heating. The silicon source is tetraethyl orthosilicate, and the amount added is greater than 0 mL and less than 15 mL.

Citation Information

Patent Citations

  • Method for preparing multistage duct zeolite molecular sieve from rice husk

    CN105731485A

  • Method for preparing SAPO-34 molecular sieve by taking rice husks as silicon source

    CN111892065A

  • A Method for Preparing ZSM-5 Zeolite by Using Solid wastes

    AU2020101871A4

  • Method for preparing hexagonal phase MCM-41 mesoporous molecular sieve from rice hull as silicon source

    CN103848435A

  • Preparation method of MFI molecular sieve of microporous-mesoporous structure

    CN107640776A