Micro-expansion anti-cracking grouting material and preparation method thereof

By using aluminate cement, silicate cement and active ultrafine mineral blends in the grouting material, the oligomer network structure is formed, which solves the problems of insufficient performance and poor durability in the early and later stages of the grouting material, and realizes the No shrinkage cracking and high durability, suitable for applications in harsh environments.

CN116177970BActive Publication Date: 2024-11-22SHANXI GUOZHENG GREEN CONSTRUCTION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310313739.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-11-22
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

The existing grouting materials have insufficient performance and strength in the early and later stages, and have a risk of shrinkage and cracking, and have poor high temperature resistance and durability, making it difficult to meet the application needs in harsh environments.

Method used

The oligomer network structure is formed by mechanical stirring and ultrasonic crushing, and the oligomer network structure is formed by mechanical stirring and ultrasonic crushing. Optimize the particle size and process to prepare a micro-expanded crack-resistant grouting material.

Benefits of technology

It achieves no shrinkage cracking, high early and late mechanical properties, good acid and water resistance, and is suitable for various harsh climate environments, extending the service life of grouting materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004149451910000021
    Figure BDA0004149451910000021
  • Figure BDA0004149451910000022
    Figure BDA0004149451910000022
  • Figure BDA0004149451910000031
    Figure BDA0004149451910000031
Patent Text Reader

Abstract

The present invention discloses a micro-expansion anti-cracking grouting material and a preparation method thereof, wherein the micro-expansion anti-cracking grouting material comprises the following components: aluminate cement, silicate cement, active ultrafine mineral admixture, alkaline activator, activator, water reducer, retarder and water; the weight proportion of each component is as follows: 20-25 parts of aluminate cement; 20-25 parts of silicate cement; 25-30 parts of active ultrafine mineral admixture; 5-8 parts of alkaline activator; 0.2-1.0 parts of activator; 0.2-1.2 parts of water reducer; 0.4-1.0 parts of retarder; 15-25 parts of water. The micro-expansion anti-cracking grouting material provided by the present invention has the characteristics of no shrinkage cracking, high early and late mechanical properties and durability, good acid resistance and water resistance, and can have extremely strong durability in various harsh climate environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a grouting material and a preparation method thereof, in particular to a micro-expansion anti-cracking grouting material and a preparation method thereof. Background Art

[0002] Grouting material is a highly fluid and plastic grouting material. Grouting material has good fluidity, can make the equipment and foundation in close contact without leaving gaps, and is resistant to aging and corrosion. Because grouting material has the characteristics of high strength, low viscosity, high fluidity, rapid hardening and good permeability, it is widely used in equipment fixation, equipment repair, equipment foundation fixing anchor bolts, high-speed rail and other projects in construction projects. In the construction industry, it is mainly used for thickening and reinforcing beams and columns, repairing cracks, reinforcing shear walls, etc.; in machinery, electricity, and wind power generation, it is mainly used for grouting anchor bolts when installing and reinforcing equipment.

[0003] Grouting materials are divided into single-component and two-component types. Common single-component grouting materials are pre-mixed in the factory and can be directly added with water on site for construction, but they have the disadvantages of long setting time and low early strength. Two-component organic grouting materials need to be mixed and configured on site. The proportion and mixing uniformity of the two components are difficult to control. After curing, its later strength is easy to shrink, and the durability of the system is poor. Grouting materials are commonly used in two grades, C40 and C60, representing its strength of 40MPa and 60Mpa respectively; they can basically meet the needs of reinforcement of concrete structures and repair of water leakage, collapse grouting of various foundation projects, and emergency repair projects. However, there is still a risk of shrinkage cracking, and the early and late performance strength still need to be improved, and the high temperature resistance and durability still need to be improved, so as to expand the application field of engineering and better meet the application in various harsh environments. Therefore, providing micro-expansion anti-cracking grouting materials has a very broad application prospect. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a micro-expansion anti-cracking grouting material and a preparation method thereof, which has the characteristics of no shrinkage cracking, higher early and late mechanical properties, good acid resistance and water resistance, and can have extremely strong durability in various harsh climatic environments.

[0005] The technical solution adopted by the present invention to solve the above technical problems is to provide a micro-expansion anti-cracking grouting material, which comprises the following components: aluminate cement, silicate cement, active ultrafine mineral admixture, alkaline activator, activator, water reducer, retarder and water.

[0006] Furthermore, the proportions of each component by weight are as follows:

[0007]

[0008] Furthermore, the active ultrafine mineral admixture is formulated in the following proportions by weight:

[0009]

[0010] Furthermore, the aluminate cement and silicate cement have finenesses of D50≤5μm and D95≤32μm, and are prepared by crushing and grading with a jet mill.

[0011] Furthermore, the fineness of the slag powder and fly ash is D50≤2μm, D97≤10μm; the particle size d50 of the steel slag powder is 12-25μm; the particle size d50 of the nickel-iron slag powder is 12-25μm; the particle size of the quartz powder is 3-10μm, and the microsilica powder is nano-grade microsilica powder.

[0012] Furthermore, the alkaline activator is one of sodium hydroxide, potassium hydroxide, calcium hydroxide, sodium metasilicate and sodium sulfate; the activator is one of tricalcium aluminate, calcium carbonate and triethanolamine; the water reducer is one of polycarboxylic acid water reducer, naphthalene water reducer, melamine water reducer, aliphatic water reducer and aminosulfonate water reducer or a combination thereof; the retarder is one of sodium citrate, sodium borate, sodium tartrate and sodium gluconate.

[0013] The present invention also provides a method for preparing the above-mentioned micro-expansion anti-cracking grouting material, which comprises the following steps: S1, mixing and stirring the active ultrafine mineral admixture and half of the water, and then adding an alkaline activator, an activator, a water reducer and a retarder according to the weight proportion of each component, and mixing the raw materials evenly by mechanical stirring; S2, continuing to add aluminate cement, silicate cement and the other half of the water and mixing; S3, using ultrasonic grinding to evenly disperse the agglomerated ultrafine solid particles in the mixed liquid to obtain the micro-expansion anti-cracking grouting material.

[0014] Furthermore, the step S1 comprises: selecting slag powder with an activity index of more than 95%, selecting secondary fly ash or primary fly ash with an activity index of more than 70%, firstly grinding by high-pressure roller until the powder particle size has a pass rate of not less than 90% at a 45 μm sieve hole, and the specific surface area of ​​the ground powder is not less than 500 m2 / kg; then crushing and grading by a jet mill to obtain ultrafine powder with a fineness of D50≤2 μm and D97≤10 μm; and then adding quartz powder, microsilicon powder, steel slag powder and nickel-iron slag powder according to the weight proportion of each component to obtain an active ultrafine mineral admixture.

[0015] Furthermore, the step S1 includes adding etching acid and grinding aid to the slag powder and fly ash, and grinding and crushing to obtain ultrafine powder with a particle size of 200-500nm.

[0016] Furthermore, the steel slag powder and nickel-iron slag powder are prepared by first crushing the steel slag and nickel-iron slag raw materials by steam kinetic energy grinding and then controlling the frequency of the classifier, and the particle size d50 is 12-25 μm.

[0017] Compared with the prior art, the present invention has the following beneficial effects: the micro-expansion anti-cracking grouting material provided by the present invention fully utilizes the advantages of rapid early strength development of sulphoaluminate cement and continuous increase in late strength of silicate cement, and combines active ultrafine mineral admixtures and alkaline activators to form an oligomer network structure to further improve strength and high temperature resistance. In addition, based on the close packing theory, the present invention optimizes the particle size, content and preparation process of each raw material, and finally obtains a micro-expansion high crack resistance grouting material with excellent performance; it has a long initial setting time, high early and late mechanical properties, good durability and high temperature resistance, and no shrinkage cracking. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the embodiments.

[0019] The micro-expansion anti-cracking grouting material for roads provided by the present invention comprises the following components: aluminate cement, silicate cement, active ultrafine mineral admixture, alkaline activator, activator, water reducer, retarder and water; the weight proportions of the components are as follows:

[0020]

[0021] It should be understood that defoamers, rheological agents, early strength agents or toughening materials can also be added to the above-mentioned formula components of the present invention. The water reducer is one of polycarboxylate water reducer, naphthalene water reducer, melamine water reducer, aliphatic water reducer and aminosulfonate water reducer or a compound thereof; preferably, the water reducer is obtained by compounding naphthalene water reducer and aliphatic water reducer in a ratio of 1:1. Naphthalene water reducer not only utilizes the double electric layer repulsion effect to achieve the dispersion of cement particles, but also its comb-shaped structure provides a steric hindrance effect, that is, the surface of cement particles is stabilized by a block or graft copolymer dispersant to prevent random agglomeration, and at the same time (OH) and (COOH) in the water reducer molecules are adsorbed on the crystal nucleus of the hydrate, which delays the crystallization and hydration hardening speed of the cement product, and is more conducive to the collapse retention of concrete. Aliphatic high-efficiency water reducer is a carbonyl pyroaldehyde synthesized by high molecular weight sulfonation. The hydrophobic main chain is aliphatic hydrocarbons. It gradually hydrolyzes in an alkaline environment, releasing functional groups with water-reducing effects, which act on the electrostatic repulsion between cement particles for a second time, thereby continuing to maintain the high fluidity of cement paste. The compounding of naphthalene-based water reducer and aliphatic-based water reducer can further improve the dispersibility and retention.

[0022] The retarder is one of sodium citrate, sodium borate, sodium tartrate and sodium gluconate; the defoamer is one of silicone defoamers and polyether defoamers. However, sodium citrate is not suitable for polycarboxylic acid water reducers. Not only does it not have a retarding effect, but it may accelerate coagulation. The mutual solubility of sodium citrate solution and polycarboxylic acid water reducers is also poor. In addition, it is generally difficult to obtain a superimposed effect when polycarboxylic acid water reducers are used in combination with other types of water reducers.

[0023] The micro-expansion anti-cracking grouting material provided by the present invention fully utilizes the advantages of rapid early strength development of sulphoaluminate cement and continuous increase in late strength of silicate cement, and combines active ultrafine mineral admixtures and alkaline activators to form an oligomer network structure to further improve strength and high temperature resistance.

[0024] The active ultrafine mineral admixture is formulated in the following proportions by weight:

[0025]

[0026] In order to ensure that the grouting material has micro-expansion and crack resistance, it is necessary to design the particles of each component to be tightly packed as a whole. Based on the theory of tight packing, when unequal-sized spheres / spheroids are tightly packed, the larger spheres will be stacked in the hexagonal and cubic most tightly packed manner, while the smaller spheres will be filled into the octahedral voids or tetrahedral voids therein according to the size of their own volumes. Since the grouting material of the present invention involves multiple components, the shapes and particle sizes of various components are different, so it is necessary to optimize the particle size, content and preparation process of each raw material so that the particle size of each component particle is fine and the particle size distribution range is narrow. In addition, the performance of various components is different. It is difficult to ensure that the particle size is well distributed in a narrow range by directly mixing and refining them together. It is necessary to optimize the particle size, content and preparation process of each raw material separately, so as to finally obtain a micro-expansion high crack resistance grouting material with excellent performance.

[0027] In the finished cement product, fine particles <3μm generally do not exceed 10%, and the content of 3-32μm particles is not less than 65%, which plays a leading role in cement strength. The more the better, and it is best not to have particles larger than 65μm. The airflow mill will classify while crushing, so that the particle crushing fineness can be uniform. The present invention can use the airflow mill to crush and classify the existing cement to obtain aluminate cement and silicate cement with fineness of D50≤5μm and D95≤32μm.

[0028] For the active ultrafine mineral admixture, the present invention selects slag powder with an activity index of more than 95%, and selects secondary fly ash or primary fly ash with an activity index of more than 70%. It first adopts high-pressure roller grinding to make the passing rate of the powder particle size at a 45μm sieve hole not less than 90%, and the specific surface area of ​​the ground powder is not less than 500㎡ / kg; and then uses a jet mill to grind and grade to obtain ultrafine powder with a fineness of D50≤2μm and D97≤10μm. Since the fly ash is in the form of spherical glass beads, the particle size distribution range of the ground slag powder is slightly smaller than that of the fly ash and there is a large range of intersection, thereby well enhancing the compaction effect during the inter-particle stacking process and improving the particle stacking density.

[0029] After the above-mentioned slag powder and fly ash are obtained, quartz powder, microsilica powder, steel slag powder and nickel-iron slag powder are added according to the weight proportion of each component to obtain an active ultrafine mineral admixture. Steel slag powder is used to increase mechanical strength, and nickel-iron slag powder is used to increase mechanical strength while eliminating the influence of electrostatic force. The particle size of the quartz powder is 3 to 10 μm, and the microsilica powder is nano-scale microsilica powder; the steel slag powder is obtained by first crushing the steel slag raw material with a steam kinetic energy mill and then controlling the frequency of the classifier, and the particle size d50 is 12 to 25 μm; the nickel-iron slag powder is obtained by first crushing the nickel-iron slag raw material with a steam kinetic energy mill and then controlling the frequency of the classifier, and the particle size d50 is 12 to 25 μm.

[0030] The present invention is described in detail and specifically by specific examples below to provide a better understanding of the present invention, but the following examples do not limit the scope of the present invention.

[0031] Example 1

[0032] The weight ratio of each component of the micro-expansion anti-cracking grouting material is:

[0033]

[0034]

[0035] The active ultrafine mineral admixture is formulated in the following proportions by weight:

[0036]

[0037] Example 2

[0038] The weight ratio of each component of the micro-expansion anti-cracking grouting material is:

[0039]

[0040] The active ultrafine mineral admixture is formulated in the following proportions by weight:

[0041]

[0042] The micro-expansion anti-cracking grouting material prepared in the above embodiment of the present invention has higher early strength and late strength than the existing grouting materials, no shrinkage cracking, good corrosion resistance, and excellent durability in various harsh climate environments. According to the standards such as "Technical Conditions for Grouting of Railway Post-Tensioning Prestressed Concrete Beam Pipe" (TB / T 3192), "Technical Specifications for Safety Appraisal of Engineering Structure Reinforcement Materials" (GB50728-2011), and "Technical Specifications for Application of Cement-based Grouting Materials" (GBT50448-2015), the physicochemical properties of the micro-expansion anti-cracking grouting material of the present invention are compared with those of ordinary grouting materials as follows:

[0043]

[0044] The test conditions for the resistance to moisture and heat aging are in an environment of 80°C and RH of 98%. After aging for 90 days, the shear strength reduction rate (%) of the steel wire rope and the grouting body (steel sleeve method) at room temperature is measured; the expansion between 3h and 24h is the expansion after hardening, and the measurement method is ASTM C 1090.

[0045] The present invention also provides a method for preparing the micro-expansion anti-cracking grouting material, the steps of which are as follows:

[0046] S1. Mix the active ultrafine mineral admixture and half of the water, then add the alkaline activator, activator, water reducer and retarder according to the weight of each component, and mix the raw materials evenly by mechanical stirring;

[0047] S2, continue to add aluminate cement, silicate cement and the other half of the water and mix;

[0048] S3. Use ultrasonic grinding to evenly disperse the agglomerated ultrafine solid particles in the mixed liquid to obtain micro-expansion anti-cracking grouting material; ultrasonic grinding is mainly used to evenly disperse the agglomerated ultrafine solid particles in the liquid and to grind the solid particles with relatively loose structure to ensure that all component particles reach the micron level.

[0049] The above components are crushed and screened before adding, so that the particle size of each component particle is relatively evenly distributed between 2 and 32 μm, so that the particles of each component can be stacked in a close-to-close manner, further improving the compressive strength. During the coagulation and hardening process, the silicon-oxygen bonds and aluminum-oxygen bonds in the raw materials are broken under the action of alkaline catalysts and then recombined to form a kind of AlO 4 and SiO 4The dense three-dimensional network structure composed of tetrahedral structural units has the characteristics of no shrinkage cracking, high strength, good durability and high temperature resistance. After the components are mixed evenly, the initial flow cone fluidity of the cementitious material is 14-18s, the initial setting time is 15-30min, the final setting time is 60-120min, the 4h compressive strength is 10-20MPa, the 1d compressive strength is 30-50MPa, and the 28d compressive strength is 60-120Mpa.

[0050] In addition, in order to improve its comprehensive performance, nano-scale microsilica powder is further added, and slag powder and fly ash can be considered to be crushed to nanometer level. Preferably, the present invention also adds etching acid and grinding aid to slag powder and fly ash, and obtains ultrafine powder with a particle size of 200-500nm after grinding and crushing, and introduces modified ultrafine powder to further increase the cohesion of the slurry. The ultrafine powder is prepared by acid etching method. On the one hand, under the condition of the same particle size, the specific surface area of ​​the particles is increased by etching micro-pits on the surface of the particles, so that the obtained concrete has better cohesion; on the other hand, the Si-O bond and Al-O bond on the surface of the particles are destroyed by etching, and the lattice is destroyed, so that the rate of ion dissolution of the obtained slag powder and fly ash after water is accelerated, and the rate of participating in the hydration reaction is accelerated, thereby obtaining better early strength. In order to avoid the etching acid affecting the subsequent alkali-induced coagulation and hardening; the retarder is preferably selected from sodium citrate or sodium gluconate with strong alkalinity. Generally speaking, ultrafine powders are easily affected by electrostatic force, van der Waals force and cohesive force during the stacking process. The addition of ultrafine conductive nickel-iron slag powder can offset part of the influence of electrostatic force. The subsequent ultrasonic crushing treatment can further reduce the influence of electrostatic force.

[0051] The micro-expansion anti-cracking grouting material obtained by the above preparation method is a self-leveling, high-strength, non-shrinkage grouting material that can meet the construction requirements in various harsh environments. It has the following characteristics:

[0052] 1. High strength and early strength: the compressive strength can reach 50Mpa in 1 day and ≥60Mpa in 3 days;

[0053] 2. Super fluid state: initial fluidity ≥300mm, can fill all gaps and meet the requirements of secondary grouting of equipment;

[0054] 3. High temperature resistance and no shrinkage: It has high temperature resistance and micro-expansion compensation functions, no shrinkage and cracking. After grouting, it ensures close contact between the equipment and the foundation, which can well meet the needs of high-precision installation.

[0055] 4. Corrosion resistance: Early-strength grouting materials are resistant to erosion and scouring. They have good resistance to sulfate and sewage erosion, and have strong scouring resistance. They can be used in projects such as seaports and sewage treatment plants.

[0056] 5. Oil resistance: After soaking in engine oil for 30 days, its strength can be increased by more than 10%.

[0057] 6. Durability: No aging, no corrosion to steel bars; 2 million fatigue tests, 50 freeze-thaw cycle tests, no significant change in strength.

[0058] As can be seen from the above, the micro-expansion anti-cracking grouting material of the present invention is an environmentally friendly and pollution-free high-performance grouting material. Compared with the existing ordinary grouting materials, the system has higher early and late mechanical properties and better durability. The present invention can obtain micro-expansion anti-cracking grouting materials with different setting times by adjusting the proportion of each component and the dosage of the retarder. The micro-expansion anti-cracking grouting material prepared by the present invention can have extremely strong durability in various harsh climate environments, further expanding the application scope of inorganic grouting materials, and the applicable scope includes: 1. Anchoring of anchor bolts and machine bases of large equipment and precision equipment; 2. Steel structures: such as rails, steel lances, steel columns, etc., which are fixed to the foundation; 3. Secondary grouting of equipment foundations; 4. Reinforcement of beams and columns, and buried steel bars; 5. Embedding of construction joints of subways, high-speed railways, and underground projects by reverse punching; 6. Reinforcement of concrete structures and repair of water leakage; 7. Collapse grouting of various foundation projects and various emergency repair projects, etc.

[0059] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make some modifications and improvements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the definition of the claims.

Claims

1. A micro-expansion anti-cracking grouting material, It is characterized in that The invention comprises the following components: aluminate cement, silicate cement, active ultrafine mineral admixture, alkaline activator, activator, water reducing agent, retarder and water; The proportions of each component by weight are as follows: 20-25 parts of aluminate cement; 20-25 parts of Portland cement; 25-30 parts of active ultrafine mineral admixture; 5-8 parts of alkaline activator; 0.2-1.0 part of active agent; Water reducing agent 0.2-1.2 parts; Retarder 0.4-1.0 part; 15-25 parts water; The active ultrafine mineral admixture is formulated in the following proportions by weight: 6-10 parts of slag powder; 5-15 parts of fly ash; 5-15 parts of quartz powder; 2-4 parts of microsilica powder; 3-6 parts of steel slag powder; 2-5 parts of nickel-iron slag powder; The water reducer is obtained by mixing a naphthalene-based water reducer and an aliphatic-based water reducer in a ratio of 1:1; the retarder is sodium citrate or sodium gluconate; and the activator is one of tricalcium aluminate, calcium carbonate and triethanolamine; The fineness of the aluminate cement and silicate cement is D50≤5μm, D95≤32μm; The fineness of the slag powder and fly ash is D50≤2μm, D97≤10μm; the particle size d50 of the steel slag powder is 12-25μm; the particle size d50 of the nickel-iron slag powder is 12-25μm; the particle size of the quartz powder is 3-10μm, and the microsilica powder is nano-scale microsilica powder.

2. The micro-expansion anti-cracking grouting material according to claim 1, It is characterized in that The aluminate cement and silicate cement are prepared by crushing and classifying with a jet mill.

3. The micro-expansion anti-cracking grouting material according to claim 1, It is characterized in that The alkaline activator is one of sodium hydroxide, potassium hydroxide, calcium hydroxide, sodium metasilicate and sodium sulfate.

4. A method for preparing the micro-expansion anti-cracking grouting material according to any one of claims 1 to 3, It is characterized in that The steps include: S1. Mix the active ultrafine mineral admixture and half of the water, then add the alkaline activator, activator, water reducer and retarder according to the weight of each component, and mix the raw materials evenly by mechanical stirring; S2, continue to add aluminate cement, silicate cement and the other half of the water and mix; S3. Ultrasonic grinding is used to evenly disperse the agglomerated ultrafine solid particles in the mixed liquid to obtain a micro-expansion anti-cracking grouting material.

5. The method for preparing the micro-expansion anti-cracking grouting material according to claim 4, It is characterized in that The step S1 comprises: selecting slag powder with an activity index of more than 95%, selecting secondary fly ash or primary fly ash with an activity index of more than 70%, firstly grinding by high-pressure roller until the passing rate of the powder particle size at a 45 μm sieve hole is not less than 90%, and the specific surface area of ​​the ground powder is not less than 500 m2 / kg; then crushing and grading by air flow mill to obtain ultrafine powder with a fineness of D50≤2 μm and D97≤10 μm; then adding quartz powder, microsilica powder, steel slag powder and nickel-iron slag powder according to the weight proportion of each component to obtain active ultrafine mineral admixture.

6. The method for preparing the micro-expansion anti-cracking grouting material according to claim 5, It is characterized in that The step S1 includes adding etching acid and grinding aid into slag powder and fly ash, and grinding and crushing to obtain ultrafine powder with a particle size of 200-500nm.

7. The method for preparing the micro-expansion anti-cracking grouting material according to claim 5 or 6, It is characterized in that The steel slag powder and nickel-iron slag powder are prepared by first crushing the steel slag and nickel-iron slag raw materials through a steam kinetic energy mill and then controlling the frequency of a classifier, and the particle size d50 is 12-25 μm.