White brominated butyl rubber plug for cosmetic packaging and preparation method thereof

Through the raw materials and process flow of specific ratios, cosmetic packaging plugs that are water-resistant and oil-resistant and white-performance are prepared, which solves the problems of glue plug performance and color matching in the existing technology, and improves product performance and market acceptance.

CN116178850BActive Publication Date: 2024-11-26HUBEI CHENNUO PHARM PACKAGING TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310148944.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-11-26
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

The prior art is difficult to prepare cosmetic packaging plugs with water and oil resistance and good white performance, especially the color matching problem with cosmetic preparations and packaging colors cannot be effectively solved.

Method used

Using brominated butyl rubber with specific ratios, calcined kaolin, polyethylene wax, titanium dioxide, magnesium oxide, zinc oxide and sulfur as raw materials, white butyl brominated butyl is prepared by stirring, intensive refining, refining and injection vulcanization molding. Rubber plug ensures that the rubber plug has water and oil resistance and high whiteness.

Benefits of technology

It realizes the water, oil resistance and high whiteness effect of cosmetic packaging plugs, improving the color matching and customer acceptance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116178850B_ABST
    Figure CN116178850B_ABST
Patent Text Reader

Abstract

The present invention discloses a white brominated butyl rubber plug for cosmetic packaging and a preparation method thereof. The white brominated butyl rubber plug for cosmetic packaging is prepared from the following raw materials by weight: 90 to 110 parts of brominated butyl rubber, 80 to 100 parts of calcined kaolin, 1 to 4 parts of polyethylene wax, 15 to 24 parts of titanium dioxide, 4 to 8 parts of magnesium oxide, 0.1 to 1 part of zinc oxide, and 0.1 to 0.5 parts of sulfur. The present invention is based on brominated butyl rubber, and by using titanium dioxide, magnesium oxide, zinc oxide, and sulfur in a specific ratio, the prepared rubber plug has water and oil resistance and also exhibits a high whiteness effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cosmetics, in particular to a white brominated butyl rubber plug for cosmetic packaging and a preparation method thereof. Background Art

[0002] At present, for the packaging plugs of cosmetics and other preparations, butyl rubber with excellent water permeability resistance is often used as the plug material in order to prevent the cosmetic preparations contained in the container from deteriorating due to water contact. However, for the packaging and storage of cosmetics, in addition to meeting the performance requirements such as water resistance and oil resistance, it is also necessary to consider the matching problem between the color of the cosmetic preparation and the color of the packaging. Packaged products with matching colors are often more popular with customers. Many existing cosmetic preparations are mostly white, and it is difficult to prepare packaging products that meet the water and oil resistance and have good white performance using the existing rubber plug preparation process. Therefore, it is necessary to propose a new rubber plug preparation process to solve the above-mentioned existing problems. Summary of the invention

[0003] The purpose of the present invention is to provide a white brominated butyl rubber stopper for cosmetic packaging and a preparation method thereof, so as to solve the problem that it is difficult to prepare a rubber stopper with water and oil resistance and good white performance in the prior art.

[0004] To solve the above technical problems, the first solution provided by the present invention is: a white brominated butyl rubber stopper for cosmetic packaging, which is made from the following raw materials, by mass: 90 to 110 parts of brominated butyl rubber, 80 to 100 parts of calcined kaolin, 1 to 4 parts of polyethylene wax, 15 to 24 parts of titanium dioxide, 4 to 8 parts of magnesium oxide, 0.1 to 1 part of zinc oxide, and 0.1 to 0.5 parts of sulfur.

[0005] Preferably, the white brominated butyl rubber plug for cosmetic packaging is made from the following raw materials, in parts by mass: 95 to 105 parts of brominated butyl rubber, 85 to 95 parts of calcined kaolin, 1 to 3 parts of polyethylene wax, 15 to 20 parts of titanium dioxide, 4 to 8 parts of magnesium oxide, 0.2 to 0.6 parts of zinc oxide, and 0.2 to 0.3 parts of sulfur.

[0006] Further preferably, the white brominated butyl rubber plug for cosmetic packaging is made from the following raw materials, in parts by mass: 100 parts of brominated butyl rubber, 89 parts of calcined kaolin, 2 parts of polyethylene wax, 18 parts of titanium dioxide, 6 parts of magnesium oxide, 0.5 parts of zinc oxide, and 0.25 parts of sulfur.

[0007] Preferably, the average brightness of the calcined kaolin is greater than 92%.

[0008] To solve the above technical problems, the second solution provided by the present invention is: a method for preparing a white brominated butyl rubber stopper for cosmetic packaging, which is used to prepare the white brominated butyl rubber stopper for cosmetic packaging in the aforementioned first solution, and comprises the following steps: S1, uniformly mixing brominated butyl rubber, calcined kaolin, polyethylene wax, titanium dioxide, magnesium oxide, zinc oxide, and sulfur in a proportion to obtain a mixture; S2, successively performing internal mixing and open mixing on the mixture to obtain a preformed body; S3, vulcanizing the preformed body by an injection vulcanization molding process, and obtaining a white brominated butyl rubber stopper for cosmetic packaging after punching and cleaning.

[0009] Wherein, in step S1, a stirrer is used for stirring and mixing, the rotation speed is 900-1100 rpm, and the stirring time is 8-15 min.

[0010] In step S2, the mixed materials in step S1 are further mixed evenly by using an internal mixer, and then introduced into an open mixer to extract the mixed materials into a preformed embryo body.

[0011] The temperature of the internal mixer is set at 80-100°C, and the outlet discharge temperature of the open mixer is set at 70-80°C.

[0012] Among them, the residence time ratio of the materials in the internal mixer and the open mixer is 1 to 1.2:1, and the total residence time of the materials in the internal mixer and the open mixer is 15 to 20 minutes.

[0013] Among them, in step S3, the conditions of the injection vulcanization molding process are: vulcanization temperature is 180-190°C, vulcanization pressure is 200-250 bar, and injection tube temperature is 70-90°C.

[0014] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides a white brominated butyl rubber plug for cosmetic packaging and a preparation method thereof. Based on brominated butyl rubber, by using titanium dioxide, magnesium oxide, zinc oxide and sulfur in a specific ratio, the prepared rubber plug has water and oil resistance while also showing a higher whiteness effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a process flow chart of an embodiment of a method for preparing a white brominated butyl rubber stopper for cosmetic packaging. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] For the first solution provided by the present invention, a white brominated butyl rubber plug for cosmetic packaging is provided, which is made from the following raw materials in parts by mass: 90-110 parts of brominated butyl rubber, 80-100 parts of calcined kaolin, 1-4 parts of polyethylene wax, 15-24 parts of titanium dioxide, 4-8 parts of magnesium oxide, 0.1-1 parts of zinc oxide, and 0.1-0.5 parts of sulfur. The preferred raw material ratio is: 95-105 parts of brominated butyl rubber, 85-95 parts of calcined kaolin, 1-3 parts of polyethylene wax, 15-20 parts of titanium dioxide, 4-8 parts of magnesium oxide, 0.2-0.6 parts of zinc oxide, and 0.2-0.3 parts of sulfur. A further preferred raw material ratio is: 100 parts of brominated butyl rubber, 89 parts of calcined kaolin, 2 parts of polyethylene wax, 18 parts of titanium dioxide, 6 parts of magnesium oxide, 0.5 parts of zinc oxide, and 0.25 parts of sulfur. Among them, the average whiteness of calcined kaolin is greater than 92%, which can keep the rubber product with a good white base color.

[0018] For the second solution provided by the present invention, please refer to Figure 1 , provides a method for preparing a white brominated butyl rubber stopper for cosmetic packaging, the method for preparing the white brominated butyl rubber stopper for cosmetic packaging in the aforementioned first solution, comprising the following steps:

[0019] S1, bromobutyl rubber, calcined kaolin, polyethylene wax, titanium dioxide, magnesium oxide, zinc oxide, and sulfur are uniformly mixed according to a proportion to obtain a mixture. In this step, a stirrer is used to stir and mix bromobutyl rubber, calcined kaolin, polyethylene wax, titanium dioxide, magnesium oxide, zinc oxide, and sulfur according to a proportion, the rotation speed is 900-1100 rpm, the stirring time is 8-15 minutes, and the mixture is obtained after stirring.

[0020] S2, the mixture is successively subjected to internal mixing and open mixing to obtain a preformed body. In this step, an internal mixer is used to further mix the mixture in step S1, and then the mixture is introduced into an open mixer to produce a preformed body; wherein the temperature of the internal mixer is set to 80-100°C, the outlet discharge temperature of the open mixer is 70-80°C, the residence time ratio of the materials in the internal mixer and the open mixer is 1-1.2:1, and the total residence time of the materials in the internal mixer and the open mixer is 15-20 minutes.

[0021] S3, vulcanize the preformed embryo body by injection vulcanization molding process, and obtain the white brominated butyl rubber plug for cosmetic packaging after punching and cleaning. In this step, the preformed embryo body is vulcanized by injection vulcanization molding process, and the conditions of injection vulcanization molding process are: vulcanization temperature 180-190°C, vulcanization pressure 200-250bar, injection tube temperature 70-90°C; after vulcanization, punching is performed as required, and then cleaned to obtain the white brominated butyl rubber plug for cosmetic packaging.

[0022] The preparation method and effect of the white bromobutyl rubber plug for cosmetic packaging in the present invention are described in detail below through specific examples. The raw materials selected in the following examples are: bromobutyl rubber BIIR2302 (Yanshan Petrochemical); calcined kaolin (Inner Mongolia Lixin); anatase titanium dioxide (Nanjing Taibai Chemical); polyethylene wax (Hebei Zhaoxian Hengxinda); sulfur powder (industrial grade); zinc oxide (Shanghai Jinghua Chemical); active magnesium oxide (Yuncheng Yaxing, Shanxi).

[0023] Example 1

[0024] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0025] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 18 parts by mass of titanium dioxide, 6 parts by mass of magnesium oxide, 0.5 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0026] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0027] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0028] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0029] Example 2

[0030] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0031] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 10 parts by mass of titanium dioxide, 6 parts by mass of magnesium oxide, 0.5 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0032] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0033] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0034] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0035] Example 3

[0036] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 30 parts by mass of titanium dioxide, 6 parts by mass of magnesium oxide, 0.5 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0037] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0038] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0039] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0040] Example 4

[0041] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0042] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 18 parts by mass of titanium dioxide, 1 part by mass of magnesium oxide, 0.5 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0043] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0044] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0045] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0046] Example 5

[0047] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0048] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 18 parts by mass of titanium dioxide, 15 parts by mass of magnesium oxide, 0.5 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0049] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0050] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0051] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0052] Example 6

[0053] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0054] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 18 parts by mass of titanium dioxide, 6 parts by mass of magnesium oxide, 0 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0055] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0056] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0057] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0058] Example 7

[0059] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0060] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 18 parts by mass of titanium dioxide, 6 parts by mass of magnesium oxide, 5 parts by mass of zinc oxide and 0.25 parts by mass of sulfur as raw materials for preparation.

[0061] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0062] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0063] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0064] Example 8

[0065] The specific steps for preparing the rubber stopper in this embodiment are as follows:

[0066] (1) Take 100 parts by mass of brominated butyl rubber, 89 parts by mass of calcined kaolin, 2 parts by mass of polyethylene wax, 18 parts by mass of titanium dioxide, 6 parts by mass of magnesium oxide, 0.5 parts by mass of zinc oxide and 2 parts by mass of sulfur as raw materials for preparation.

[0067] (2) The above raw materials were stirred and mixed using a stirrer at a rotation speed of 1000 rpm for 10 min to obtain a mixture.

[0068] (3) The above-mentioned mixture is further mixed uniformly by using an internal mixer, the temperature of the internal mixer is set to 90° C., and the residence time of the materials in the internal mixer is 8 minutes; then the mixed material is introduced into an open mixer to produce a preformed embryo, the outlet discharge temperature of the open mixer is 75° C., and the residence time of the materials in the open mixer is 8 minutes.

[0069] (4) The preformed body is vulcanized by injection vulcanization molding process, the vulcanization temperature is 180°C, the vulcanization pressure is 220 bar, and the injection tube temperature is 70°C (the specific test is the tube body temperature); after the vulcanization is completed, punching is performed as required, and then cleaned to obtain a rubber plug sample.

[0070] The rubber stopper samples prepared in Examples 1 to 8 were subjected to oil resistance test (mineral oil infiltration at room temperature, testing whether the mass change rate after 30 days of infiltration is greater than 5%), moisture permeability test (water infiltration at room temperature, testing whether the mass change rate after 30 days of infiltration is greater than 5%) and whiteness value test, and the results are shown in Table 1.

[0071] Table 1

[0072] Is the oil-infiltrated mass change rate greater than 5%? Is the water infiltration mass change rate greater than 5%? Whiteness / % Example 1 no no 96.5 Example 2 no no 93.5 Example 3 no no 93.1 Example 4 no no 94.1 Example 5 no no 94.2 Example 6 no no 93.8 Example 7 no no 92.3 Example 8 Yes (Oil-wetted mass change rate 6.3%) Yes (Water infiltration mass change rate 6.8%) 95.2

[0073] As can be seen from Table 1, the titanium dioxide content in Examples 2 and 3 is less or more than that in Example 1, the magnesium oxide content in Examples 4 and 5 is less or more than that in Example 1, and the zinc oxide content in Examples 6 and 7 is less or more than that in Example 1. The less or more content of titanium dioxide, magnesium oxide, and zinc oxide has little effect on the oil and water resistance of the prepared rubber plug, while the less or more content of titanium dioxide, magnesium oxide, and zinc oxide has a significant effect on the whiteness of the prepared rubber plug, indicating that the prepared rubber plug can only show a better whiteness value when titanium dioxide, magnesium oxide, and zinc oxide meet a specific ratio. In addition, the whiteness value of the rubber plug prepared in Example 1 is higher than the whiteness value of the existing commercially available rubber plugs.

[0074] It can be seen from Table 1 that the sulfur content in Example 8 is higher than that in Example 1, which will affect the subsequent vulcanization molding process, resulting in little effect on the whiteness effect and a greater impact on the oil and water resistance. Therefore, the sulfur in the raw material also needs to meet the aforementioned limited range to obtain better results.

[0075] Different from the prior art, the present invention provides a white brominated butyl rubber plug for cosmetic packaging and a preparation method thereof. Based on brominated butyl rubber, by adopting titanium dioxide, magnesium oxide, zinc oxide and sulfur in a specific ratio, the prepared rubber plug has water and oil resistance and also exhibits a high whiteness effect.

[0076] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For details not described in individual embodiments, reference may be made to the description in other embodiments.

[0077] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A white bromobutyl rubber stopper for cosmetic packaging, It is characterized in that The invention is prepared from the following raw materials, in parts by mass: 90-110 parts of brominated butyl rubber, 80-100 parts of calcined kaolin, 1-4 parts of polyethylene wax, 15-24 parts of titanium dioxide, 4-8 parts of magnesium oxide, 0.1-1 parts of zinc oxide, and 0.1-0.5 parts of sulfur, wherein the average whiteness of the calcined kaolin is greater than 92%.

2. The white brominated butyl rubber stopper for cosmetic packaging according to claim 1, It is characterized in that The invention is prepared from the following raw materials, by weight: 95-105 parts of brominated butyl rubber, 85-95 parts of calcined kaolin, 1-3 parts of polyethylene wax, 15-20 parts of titanium dioxide, 4-8 parts of magnesium oxide, 0.2-0.6 parts of zinc oxide, and 0.2-0.3 parts of sulfur.

3. The white brominated butyl rubber stopper for cosmetic packaging according to claim 1, It is characterized in that The invention is prepared from the following raw materials, by weight: 100 parts of brominated butyl rubber, 89 parts of calcined kaolin, 2 parts of polyethylene wax, 18 parts of titanium dioxide, 6 parts of magnesium oxide, 0.5 parts of zinc oxide, and 0.25 parts of sulfur.

4. A method for preparing a white brominated butyl rubber stopper for cosmetic packaging as claimed in any one of claims 1 to 3, It is characterized in that The steps include: S1, mixing bromobutyl rubber, calcined kaolin, polyethylene wax, titanium dioxide, magnesium oxide, zinc oxide and sulfur in a uniform ratio to obtain a mixture; S2, the mixed material is subjected to internal mixing and open mixing in sequence to obtain a preformed body; S3, vulcanizing the preformed embryo body by injection vulcanization molding process, and obtaining the white brominated butyl rubber plug for cosmetic packaging after punching and cleaning.

5. The method for preparing the white brominated butyl rubber stopper for cosmetic packaging according to claim 4, It is characterized in that In the step S1, a stirrer is used for stirring and mixing, the rotation speed is 900-1100 rpm, and the stirring time is 8-15 min.

6. The method for preparing the white brominated butyl rubber stopper for cosmetic packaging according to claim 4, It is characterized in that In the step S2, the mixed materials in the step S1 are further mixed evenly by using an internal mixer, and then introduced into an open mixer to mix and output the mixed materials into a preformed embryo body.

7. The method for preparing the white brominated butyl rubber stopper for cosmetic packaging according to claim 6, It is characterized in that The temperature of the internal mixer is set at 80-100°C, and the outlet discharge temperature of the open mixer is 70-80°C.

8. The method for preparing the white brominated butyl rubber stopper for cosmetic packaging according to claim 6, It is characterized in that The residence time ratio of the materials in the internal mixer and the open mixer is 1-1.2:1, and the total residence time of the materials in the internal mixer and the open mixer is 15-20 min.

9. The method for preparing the white brominated butyl rubber stopper for cosmetic packaging according to claim 4, It is characterized in that In the step S3, the conditions of the injection vulcanization molding process are: vulcanization temperature of 180-190° C., vulcanization pressure of 200-250 bar, and injection tube temperature of 70-90° C.

Citation Information

Patent Citations

  • Brominated butyl rubber plug and preparation method thereof

    CN104744834A