An aqueous radioactive anion adsorbent based on anion-π interaction

The porous network framework material uses multiple anion-π interactions to solve the problem of separation and enrichment of radioactive anions in water, achieving efficient, economical, and environmentally friendly radioactive anion adsorption and separation, and is suitable for the treatment of low-concentration pollutants in water.

CN116196903BInactive Publication Date: 2024-10-18CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310286542.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively handle low-concentration radioactive anions in water, especially 99Tc, 188Re and 131I, and conventional methods are inefficient and complex, making it difficult to achieve selective separation and enrichment.

Method used

It uses a porous network skeleton material formed by connecting bicyclic calixarene building molecules with a cage-like structure to metal ions. It achieves efficient adsorption and selective separation of radioactive anions through multiple anion-π interactions. The material preparation cost is low, the operation is simple, and it is environmentally friendly. friendly.

Benefits of technology

It achieves high adsorption capacity, easy recovery, high selectivity and high stability for TcO4-, ReO4-, IO4- and other oxygen-containing acid radicals. The anion concentration in the treated water is reduced to less than 1ppm, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116196903B_ABST
    Figure CN116196903B_ABST
Patent Text Reader

Abstract

The present invention discloses a network framework material suitable for selective separation and enrichment of radioactive anions in aqueous phase. This material is a porous network framework structure formed by the coordination of bicyclic calixarene building block molecules and metal ions, and has nano-micropores formed by electron-deficient aromatic rings. The micropores can separate radioactive TcO4 through multiple anion-π interactions. ‑ , ReO4 ‑ ,IO4 ‑ The selective recognition and combination of oxygen-containing anions can effectively remove radioactive oxygen-containing anions with a concentration of 1-2000ppm in water, and has the characteristics of large adsorption capacity and fast kinetics. Under the conditions of the presence of competitive anions and different anion concentrations in water, its adsorption efficiency can reach more than 90%. At the same time, this type of material is easy to recycle and regenerate, and its radioactive anion separation and enrichment efficiency can be well maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radioactive element separation and treatment, and in particular relates to a material suitable for selective separation and enrichment of radioactive anions in an aqueous phase. The material can achieve efficient recognition and selective separation of radioactive anions through anion-π interaction. Background Art

[0002] With the development of modern industry and economy, the amount of wastewater discharged and pollutants has increased rapidly. The problem of anion pollution in wastewater is also becoming more and more serious. Many different heavy metal anions are of great significance to public health and safety due to their high toxicity. In recent years, radioactive perrhenate, pertechnetate, periodate and other oxygen-containing acid anions have attracted widespread attention due to the rapid increase in environmental water discharge. 99 Tc, 188 Re, 131 I has a wide range of uses in radioactive medical diagnosis. 99 Tc has a very long half-life (2.1×10 5 Years) and good environmental mobility, the output is increasing every year due to the development of the nuclear industry. Ion exchange and reduction immobilization are currently the conventional methods used to remove these anions, but these methods have problems such as low efficiency, complex post-treatment, and difficulty in effectively treating low-concentration radioactive anions. The development of anion adsorption materials with high adsorption capacity, fast kinetics and selectivity is the key to solving such radioactive anion pollution problems. However, anions usually have a relatively large volume and a low charge / surface ratio, and the design and development of related materials is very challenging due to the lack of strong anion binding sites. Heterogeneous adsorption materials are easy to regenerate and reuse, and can better meet the needs of practical industrial applications.

[0003] Anion-π interaction is a new type of weak non-covalent interaction that was proposed in this century and has only recently attracted attention. Although the strength of the anion-π interaction is very weak, there have been no previous reports showing that this force can be used for the selective recognition and enrichment of anions in the aqueous phase. Based on the basic principles of supramolecular chemistry, we believe that constructing a cavity with multiple anion-π interactions is a different strategy to achieve the separation and enrichment of radioactive anions. Summary of the invention

[0004] The purpose of the present invention is to provide a kind of material suitable for selective separation and enrichment of radioactive anions in water phase, which has the characteristics of low preparation cost, simple operation, environmental friendliness, economic efficiency, and at the same time, this kind of material has good performance in natural environment conditions. - , ReO4 - ,IO4 - Oxygen-containing acid radicals have the advantages of high adsorption capacity, easy recovery, high selectivity and high stability.

[0005] In the present invention, the above-mentioned material suitable for selective separation and enrichment of radioactive anions in an aqueous phase is a porous network skeleton structure formed by the coordination of a bicyclic calixarene building block molecule with a cage structure and a metal ion linker. The cyclocalixarene building block molecule is composed of a three-dimensional structure with D3h symmetry and three side arms constructed by electron-deficient aromatic rings, and the electron-deficient aromatic ring (Ar) can be a five-membered dinitrogen aromatic heterocycle (I), a triazole ring (II), a six-membered dinitrogen aromatic heterocycle (III), a six-membered trinitrogen aromatic heterocycle (IV), a triazine-linked six-membered mononitrogen aromatic heterocycle (V), a triazine-linked six-membered dinitrogen aromatic heterocycle (VI), a triazine-linked six-membered trinitrogen aromatic heterocycle (VII), a triazine-linked five-membered dinitrogen aromatic heterocycle (VIII), and a triazine-linked triazole ring (IX).

[0006]

[0007] The metal ion linkers mentioned above are transition metal ions with 6-coordination capacity, including: Fe 2+ ,Co 2+ , Ni 2+ , Cu 2+ , Zn 2+ , Cd 2+ , Mn 2+ , Fe 3+ ,Cr 3+ ,Co 3+ .

[0008] The above-mentioned bicyclic calix aromatic building block molecules and soluble salts of metal ions (nitrates, perchlorates or sulfates) are added into a glass bottle at a ratio of 1:3-10, and an appropriate amount of N,N-dimethylformamide (or DMSO, N,N-diethylformamide) is added to dissolve. After sealing, the bottle is heated at 60-120°C for 3-48 hours and then slowly cooled to precipitate the corresponding crystal network skeleton material.

[0009] The present invention also provides the use of the porous network skeleton material in removing radioactive anions in water phase, comprising: loading the crystal network skeleton material into a filling column, and adding the aqueous solution to be treated containing radioactive oxygen-containing acid anions from the top of the filling column.

[0010] Furthermore, the porous network skeleton material has an electron-deficient cavity structure.

[0011] Furthermore, the crystal structure showed that the network framework binds radioactive oxoacid anions through multiple anion-π interactions.

[0012] Furthermore, the total content of radioactive oxygen-containing acid anions in the aqueous solution to be treated does not exceed 80% of the theoretical maximum adsorption capacity of the filling crystal material.

[0013] Furthermore, the porous network framework material still has high selectivity for target radioactive anions in the presence of excess competing anions.

[0014] Furthermore, the porous network skeleton material has high stability in the aqueous solution to be treated.

[0015] Furthermore, the porous network skeleton material can be recycled by soaking in perchlorate after adsorption and separation.

[0016] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:

[0017] (1) The radioactive anion adsorption material disclosed in the present invention realizes the selective binding and adsorption of target anions through multiple anion-π interactions.

[0018] (2) The anion adsorption material disclosed in the present invention is easy to synthesize, simple to operate, recyclable, and can be applied on a large scale.

[0019] (3) The anion adsorption material disclosed in the present invention can selectively bind to radioactive oxygen-containing acid anions to achieve selective adsorption and separation of related radioactive anions in wastewater.

[0020] (4) The anion adsorption material disclosed in the present invention can achieve an adsorption effect of up to 99% on radioactive oxygen-containing acid anions in aqueous solution, reducing the anion concentration in the treated water to below 1 ppm, and has high stability and recyclability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Contains Zn 2+ Single crystal structure diagram of porous network skeleton material.

[0022] Figure 2 Contains Cd 2+ Single crystal structure diagram of porous network skeleton material.

[0023] Figure 3 Contains Zn 2+ Comparison of infrared spectra of porous network skeleton materials before and after adsorption. A is the Zn-containing 2+ Infrared spectrum of porous network skeleton material before adsorption, B is Zn 2+ Porous network skeleton material adsorbs ReO4 - After infrared spectrum, C is Zn 2+ Infrared spectrum of the porous network skeleton material after recovery.

[0024] Figure 4 Contains Zn 2+ Porous network skeleton materials for ReO4 - Schematic diagram of the cyclic adsorption effect.

[0025] Figure 5 Contains Cd 2+ Porous network skeleton materials for ReO4 - Schematic diagram of the cyclic adsorption effect.

[0026] Figure 6 Contains Zn 2+ Porous network skeleton materials for IO4 - Schematic diagram of the cyclic adsorption effect.

[0027] Figure 7 Contains Zn 2+ Porous network skeleton materials for TcO4 - Schematic diagram of the cyclic adsorption effect.

[0028] Figure 8 Contains Zn 2+ Porous network framework materials for ReO4 under the coexistence of competing anions - Adsorption effect diagram. DETAILED DESCRIPTION

[0029] The technical scheme of the present invention is described clearly and completely below in conjunction with the embodiments. The described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0030] Example 1: Preparation of bicyclic calixarene building block molecule 1 with a cage structure, the specific steps are as follows:

[0031] 0.03 mol of 2,4-dichloro-1,3,5-triazine and 0.02 mol of phloroglucinol were added to a flask, and then 0.06 mol of potassium carbonate and 100 mL of dimethyl sulfoxide were added as solvent, and stirred at 100°C for 6 hours. After the reaction was completed, water was added to stop the reaction, and the mixture was extracted with ethyl acetate, dried, concentrated, and purified by column chromatography to obtain the bicyclic calixarene building block molecule 1.

[0032]

[0033] Example 2: Preparation of bicyclic calixarene building block molecule 2 with cage structure is the same as Example 1, but the difference is that 2,4-dichloro-1,3,5-triazine is replaced by 4,6-dichloropyrimidine.

[0034] Example 3: Preparation of bicyclic calixarene building block molecule 3 with cage structure The preparation was the same as in Example 1, except that 2,4-dichloro-1,3,5-triazine was replaced by 2,6-dichloropyrazine.

[0035] Example 4: The preparation of bicyclic calixarene building block molecule 4 with a cage-like structure is the same as in Example 1, except that 2,4-dichloro-1,3,5-triazine is replaced by 3,5-dichloropyridazine.

[0036] Example 5: Preparation of bicyclic calixarene building block molecule 5 with a cage structure, the specific steps are as follows:

[0037] Step 1: 0.015 mol of phloroglucinol and 0.05 mol of N,N-diisopropylethylamine (DIPEA) were dissolved in 50-60 mL of tetrahydrofuran. In an argon-protected ice-water bath, the mixture was added dropwise to 100 mL of a tetrahydrofuran solution containing 0.065 mol of cyanuric chloride. After reacting in the ice-water bath for 1 hour, the residue was removed by filtration, the filtrate was concentrated, and the intermediate 1 was purified by column chromatography.

[0038]

[0039] Step 2: 0.01 mol of intermediate 1 and 0.01 mol of phloroglucinol were dissolved in 100 mL of acetone, 200 mL of acetone and 0.07 mol of DIPEA were added to a three-necked flask, and the acetone solution containing intermediate 1 and phloroglucinol was added dropwise to the three-necked flask at the same speed, and the reaction was carried out for 3 days. After the reaction was completed, intermediate 2 was purified by column chromatography.

[0040]

[0041] Step 3: 0.06 mol imidazole, 0.06 mol DIPEA and 50 mL tetrahydrofuran were added to the flask, 0.01 mol intermediate 2 was dissolved in 60 mL tetrahydrofuran, and added dropwise to the flask for 3 hours. After the reaction, the residue was filtered and separated, and the residue was washed once with water and three times with ethanol, and dried to obtain the bicyclic calixarene building block molecule 5.

[0042]

[0043] Example 6: Preparation of bicyclic calixarene building block molecule 6 with a cage structure, the specific steps are as follows:

[0044] Step 1: 0.03 mol of cyanuric chloride and 0.01 mol of 4-bromopyridine were added to a reaction bottle, and then 0.0002 mol of palladium acetate and 120 mL of N,N-dimethylformamide were added and stirred to dissolve, and then 0.03 mol of potassium phosphate aqueous solution was added and heated to 120°C for overnight reaction. After the reaction was completed, the solvent was removed and the mixture was purified by column chromatography to obtain 2-(4-pyridyl)-4,6-dichlorotriazine.

[0045]

[0046] Step 2: Add 0.015 mol of 2-(4-pyridyl)-4,6-dichlorotriazine, 0.01 mol of phloroglucinol and 0.03 mol of cesium carbonate into a flask, use dimethyl sulfoxide as solvent, and react at room temperature for 6 hours. Add water to stop the reaction, and extract with ethyl acetate. After drying and concentration, purify by column chromatography to obtain bicyclic calixarene building block molecule 6.

[0047]

[0048] Example 7: Containing Zn 2+ The preparation of porous network skeleton materials, the specific steps are as follows:

[0049] The bicyclic calixarene building block molecule 5 and zinc perchlorate hexahydrate were added into a bottle in a ratio of (1:5), and an appropriate amount of N,N-dimethylformamide was added to dissolve the mixture. The mixture was heated at 120°C for 0.5 hours, and then cooled naturally. The corresponding crystals were precipitated within three days. After drying, the Zn-containing 2+ Porous network skeleton material.

[0050] Determination of Zn content by X-ray single crystal diffraction 2+ The crystal structure of porous network skeleton materials, Figure 1 Contains Zn 2+ Single crystal structure diagram of porous network skeleton material, composed of Figure 1 a This shows that Zn 2+ The porous network skeleton material has a layered structure. Figure 1 b is Zn 2+ The inner layer structure of the porous network skeleton material is shown in Figure 1. Figure 1 b Visible, containing Zn 2+ The porous network skeleton material has three V-shaped cavities formed by two electron-deficient triazine ring side arms. The V-shaped cavities in the layer contain perchlorate (ClO4 - ).

[0051] Example 8: Containing Cd 2+ The preparation of the porous network skeleton material is the same as in Example 7, except that zinc perchlorate hexahydrate is replaced with cadmium nitrate tetrahydrate. 2+The crystal structure of porous network skeleton materials, Figure 2 Contains Cd 2+ Single crystal structure diagram of porous network skeleton material, Figure 2 a shows the Cd 2+ The layered structure of porous network skeleton materials, Figure 2 b shows the structure of the layer, which shows that the Cd 2+ The porous network framework material also has a V-shaped cavity formed by electron-deficient triazine rings.

[0052] Example 9: Containing Co 2+ The preparation of the porous network skeleton material is the same as that of Example 7, except that zinc perchlorate hexahydrate is replaced with cobalt nitrate hexahydrate.

[0053] Example 10: Containing Ni 2+ The preparation of porous network skeleton materials, the specific steps are as follows:

[0054] The bicyclic calixarene building block molecule 6 and nickel sulfate (II) hexahydrate were added into the bottle in a ratio of (1:8), and an appropriate amount of N,N-dimethylformamide was added to dissolve, and the mixture was heated at 120°C for 24 hours, and then naturally cooled. The corresponding crystals were precipitated within three days, and the Ni-containing 2+ Porous network skeleton material.

[0055] Example 11: Containing Fe 2+ The preparation of the porous network skeleton material is the same as in Example 10, except that nickel sulfate (II) hexahydrate is replaced by ferrous chloride tetrahydrate.

[0056] Example 12: Containing Zn 2+ Porous network skeleton materials for ReO4 - The specific steps of the adsorption experiment are as follows:

[0057] Ammonium perrhenate was dissolved in DMF to prepare an ammonium perrhenate DMF solution with a Re content of 1000 ppm. 2+ The porous network skeleton material was immersed in ammonium perrhenate DMF solution for one day. The adsorbed Zn content was detected by single crystal X-ray diffraction. 2+ The crystal structure of the porous network skeleton material shows that it originally contained Zn 2+ ClO4 contained in the electron-deficient V-shaped cavity in the porous network skeleton material crystal structure - All replaced by ReO4 - The network skeleton binds ReO4 through multiple anion-π interactions - .

[0058] Example 13: Containing Zn 2+ Porous network skeleton material to different concentrations of ReO4 -The specific steps of the adsorption experiment are as follows:

[0059] Prepare aqueous ammonium perrhenate solutions with different concentrations, Re contents of 5ppm, 10ppm, 20ppm, 50ppm, 100ppm, 200ppm, 400ppm, and 800ppm. Take 5mg of dry Zn-containing 2+ The porous network skeleton material is filled into the chromatography column. Take 5 mL of ammonium perrhenate aqueous solution and add it to the Zn 2+ The porous network skeleton material filled column was used for adsorption experiment, and 5 mL of ammonium perrhenate aqueous solution flowed through the filled column for 30 minutes. The residual Re content in the solution after passing through the chromatography column was detected by inductively coupled plasma mass spectrometry, and the Langmuir adsorption curve was drawn, and the maximum adsorption amount of rhenium element was 130.04 mg / g.

[0060] Figure 3 Contains Zn 2+ Comparison of infrared spectra of porous network skeleton materials before and after adsorption. A is the Zn-containing 2+ Infrared spectrum of porous network skeleton material before adsorption, B is Zn 2+ Porous network skeleton material adsorbs ReO4 - After infrared spectrum, C is Zn 2+ Infrared spectrum of the porous network skeleton material after recovery. Figure 3 It can be seen that Zn 2+ Porous network skeleton material adsorbs ReO4 - After 914.09cm -1 The characteristic peak of perrhenate appeared at 2+ The characteristic peak of perrhenate in the porous network skeleton material disappears, and the infrared spectrum before adsorption Figure 1 The above results show that Zn 2+ The porous network skeleton material has good stability even after multiple adsorption and recycling processes.

[0061] Example 14: Containing Cd 2+ Porous network skeleton material to different concentrations of ReO4 - The specific steps of the adsorption experiment are the same as those of Example 13, but the difference is that the Zn-containing 2+ The porous network skeleton material is replaced with Cd 2+ Porous network skeleton material.

[0062] Example 15: Containing Zn 2+ Porous network skeleton materials for ReO4 - The specific steps are as follows:

[0063] Prepare ammonium perrhenate aqueous solution with Re content of 200ppm. Contains Zn2+ After the porous network skeleton material is dried, 50 mg is taken and filled into the chromatography column. 5 mL of ammonium perrhenate aqueous solution is added to the Zn-containing 2+ The porous network skeleton material filled column was used for adsorption experiment, and 5 mL of ammonium perrhenate aqueous solution flowed through the filled column for 30 min. 2+ Porous network skeleton material 1.73x10 -2 mol / L potassium perchlorate aqueous solution was soaked for 12 hours, filtered and dried for recovery. After simple recovery, 50 mg was taken to fill the chromatography column and the cycle experiment was carried out five times. The Re content remaining in the solution after passing through the chromatography column was detected by inductively coupled plasma mass spectrometry.

[0064] Figure 4 Contains Zn 2+ Porous network skeleton material for ReO4 at room temperature and pressure - The cyclic adsorption effect diagram. During the 5 adsorption experiments, ReO4 - The removal effect of Zn 2+ The porous network skeleton material has good recycling performance.

[0065] Example 16: Containing Cd 2+ Porous network skeleton materials for ReO4 - The cyclic adsorption performance experiment was carried out in the same manner as in Example 15, except that the Zn-containing 2+ The porous network skeleton material is replaced with Cd 2+ Porous network skeleton material. Figure 5 Contains Cd 2+ Porous network skeleton material for ReO4 at room temperature and pressure - Schematic diagram of the cyclic adsorption effect.

[0066] Example 17: Containing Zn 2+ Effect of porous network skeleton materials on different concentrations of IO4 - The specific steps of the adsorption experiment are as follows:

[0067] Prepare potassium periodate aqueous solution with I content of 5ppm, 20ppm, 50ppm, 200ppm, 400ppm, 800ppm, take 50mg of dry Zn-containing 2+ The porous network skeleton material is filled into the chromatography column. 5 mL of potassium periodate aqueous solution is added to the Zn 2+ The porous network skeleton material filled column was used for adsorption experiment, and 5 mL potassium periodate aqueous solution flowed through the filled column for 30 min. 2+ Porous network skeleton material 1.73x10 -2The solution was immersed in a 100 mol / L potassium perchlorate aqueous solution for 12 hours, filtered, dried and recovered. The residual I content in the solution after passing through the chromatography column was detected by inductively coupled plasma mass spectrometry.

[0068] Example 18: Containing Cd 2+ Effect of porous network skeleton materials on different concentrations of IO4 - The specific steps of the adsorption experiment are the same as those of Example 17, but the difference is that the Zn-containing 2+ The porous network skeleton material is replaced with Cd 2+ Porous network skeleton material.

[0069] Example 19: Containing Zn 2+ Porous network skeleton materials for IO4 - The specific steps are as follows:

[0070] Prepare potassium periodate aqueous solution with I content of 100ppm. 2+ After the porous network skeleton material is dried, 50 mg is taken and filled into the chromatography column. 5 mL of potassium periodate aqueous solution is added to the Zn-containing 2+ The porous network skeleton material filled column was used for adsorption experiment, and 5 mL potassium periodate aqueous solution flowed through the filled column for 30 min. 2+ Porous network skeleton material 1.73x10 -2 mol / L potassium perchlorate aqueous solution for 12 hours, filtered and dried for recovery. After simple recovery, 50 mg was taken to fill the chromatography column and the cycle experiment was carried out five times. The residual I content in the solution after passing through the chromatography column was detected by inductively coupled plasma mass spectrometry. Figure 6 Contains Zn 2+ Porous network skeleton materials for IO4 - Schematic diagram of the cyclic adsorption effect.

[0071] Example 20: Containing Zn 2+ Porous network skeleton materials for TcO4 - The specific steps of the cyclic adsorption experiment are as follows:

[0072] Prepare sodium pertechnetate aqueous solution with Tc content of 20ppm. 2+ After the porous network skeleton material is dried, 10 mg is taken and filled into the chromatography column. 5 mL of sodium pertechnetate aqueous solution is added to the Zn-containing 2+ The porous network skeleton material filled column was used for adsorption experiment, and 5 mL of sodium pertechnetate aqueous solution flowed through the filled column for 30 min. 2+ Porous network skeleton material 1.73x10 -2mol / L potassium perchlorate aqueous solution for 12 hours, filtered and dried for recovery. After simple recovery, 10 mg was filled into the chromatography column and the cycle experiment was repeated five times. The Tc content remaining in the solution after passing through the chromatography column was detected by inductively coupled plasma mass spectrometry. Figure 7 Contains Zn 2+ Porous network skeleton materials for TcO4 - Schematic diagram of the cyclic adsorption effect.

[0073] In fact, nuclear waste also contains SO4 2- 、NO3 - PO4 3- , Cl - Br - ,I - Therefore, it is necessary to investigate the effect of porous network skeleton materials on ReO4 when multiple anions coexist. - adsorption performance.

[0074] Example 21: When multiple anions coexist, Zn 2+ Porous network skeleton materials for ReO4 - The adsorption performance experiment of MgCl2O3 was carried out as follows:

[0075] Prepare a solution containing equal amounts of substances (1.5×10 -3 mol / L) NH4ReO4, NaH2PO4, Na2SO4, KNO3, KBr, NaCl mixed solution, rhenium content is 280ppm. Contains Zn 2+ After the porous network skeleton material is dried, 10 mg is taken and filled into the chromatography column. 4 mL of the mixed solution is added to the column containing Zn 2+ The adsorption experiment was carried out in the chromatography column of the porous network skeleton material, and 4 mL of the mixed solution flowed through the chromatography column for 30 min. 2+ Porous network skeleton material 1.73x10 -2 mol / L potassium perchlorate aqueous solution for 12 hours, filtered and dried for recovery. After simple recovery, 50 mg was filled into the chromatography column and the cycle experiment was repeated 4 times. The ReO4 remaining in the solution after passing through the chromatography column was detected by inductively coupled plasma mass spectrometry. - concentration.

[0076] Figure 8 Contains Zn 2+ Porous network framework materials for ReO4 under the coexistence of competing anions - The cyclic adsorption effect diagram. According to the maximum adsorption capacity, 10mg Zn 2+The porous network skeleton material can adsorb 1.3 mg of rhenium. The total mass of rhenium in 4 mL of a mixed solution with a rhenium content of 280 ppm is 1.12 mg. That is, under the condition that the maximum adsorption amount does not exceed 90% and other anions coexist, the content of Zn 2+ Porous network skeleton materials for ReO4 - The adsorption capacity of Zn 2+ Porous network skeleton materials for ReO4 - The adsorption selectivity is high, it is not affected by other anions, and has good cycle performance.

[0077] Example 22: When multiple anions coexist, Cd 2+ Porous network skeleton materials for ReO4 - The adsorption performance experiment was carried out in the same manner as in Example 21, except that the Zn-containing 2+ The porous network skeleton material is replaced with Cd 2+ Porous network skeleton material.

Claims

1. A material suitable for selective separation and enrichment of radioactive anions in aqueous phase based on anion-π interaction, characterized in that: The porous network skeleton structure is formed by the bicyclic calixarene building block molecules with a cage structure and the metal ions coordinated and connected. The network skeleton structure has nano-sized micropores surrounded by electron-deficient aromatic rings, which can selectively recognize and bind to the radioactive oxygen-containing acid anion TcO4 - 、ReO4 - or IO4 - , selectively bind anions through multiple anion-π interactions; The bicyclic calixarene building block molecule has D 3h The invention discloses a symmetrical three-dimensional structure and three side arms constructed by electron-deficient aromatic rings, wherein the electron-deficient aromatic ring Ar ring is a five-membered dinitrogen aromatic heterocycle (I), a triazole ring (II), a six-membered dinitrogen aromatic heterocycle (III), a six-membered trinitrogen aromatic heterocycle (IV), a triazine-linked six-membered mononitrogen aromatic heterocycle (V), a triazine-linked six-membered dinitrogen aromatic heterocycle (VI), a triazine-linked six-membered trinitrogen aromatic heterocycle (VII), a triazine-linked five-membered dinitrogen aromatic heterocycle (VIII) or a triazine-linked triazole ring (IX); the metal ion is a transition metal ion Fe with a 6-coordination capacity. 2+ 、Co 2+ 、Ni 2+ , Cu 2+ 、Zn 2+ 、Cd 2+ , Mn 2+ , Fe 3+ Cr 3+ or Co 3+ ; 。 2. A method for preparing a material suitable for selective separation and enrichment of radioactive anions in an aqueous phase based on anion-π interaction according to claim 1, characterized in that: Add a bicyclic calixarene building block compound and a metal salt in a ratio of 1:3-10 into a glass bottle, add an appropriate amount of solvent to dissolve, seal the bottle, heat at 60-120°C for 0.1-48 hours, and then slowly cool down to precipitate a corresponding crystal network skeleton material; the salt is nitrate, perchlorate or sulfate; the solvent is N,N-dimethylformamide, DMSO or N,N-diethylformamide.

3. An application of the material for selective separation and enrichment of radioactive anions in aqueous phase based on anion-π interaction according to claim 1, characterized in that: The crystal material is loaded into a filling column, and an aqueous solution containing radioactive oxygen-containing acid anions is added from the top of the filling column. The content of anions in the water does not exceed 90% of the theoretical maximum adsorption capacity of the filled crystal material. The content of radioactive anions to be treated in the water ranges from 1 to 2000 mg / L, and 1 to 10 equivalents of other anions are allowed. The other anions are Cl - Br - ,I - 、NO3 - 、H2PO4 - or SO4 2- The adsorbent material is used after use with high concentration ClO4 - After being activated by solution immersion and reuse, the performance can still be maintained at more than 90% after 4 cycles.