Hydrogenation catalyst and its preparation method and application

By using a heat treatment process of carbon carrier precursor and phosphorus source in the preparation of mesoporous carbon materials, combined with the introduction of metal elements, the problems of complex processes and high costs in the existing technology are solved, and low-cost, environmentally friendly mesoporous carbon materials are achieved. Preparation and production of efficient hydrogenation catalysts.

CN116196956BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111444896.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2024-10-15
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

The existing preparation process of mesoporous carbon materials is complex and requires acid or alkali washing to produce waste liquid. The use of organic templates is costly and difficult to be suitable for large-scale industrial applications.

Method used

The carbon carrier precursor and the phosphorus source are heat treated in an oxygen-containing atmosphere, and the uniformly mixed mixture is heat treated to prepare a mesoporous carbon carrier, and Group VIII metal elements and Group VIB metal elements are introduced to form a supported type Hydrogenation catalyst.

Benefits of technology

The low-cost and environmentally friendly preparation of mesoporous carbon materials is achieved, which is suitable for industrial large-scale production and improves the hydrogenation activity of the hydrogenation catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003384632630000161
    Figure BDA0003384632630000161
  • Figure BDA0003384632630000171
    Figure BDA0003384632630000171
Patent Text Reader

Abstract

The present invention discloses a hydrogenation catalyst and a preparation method and application thereof, wherein the catalyst comprises a mesoporous carbon carrier and an active metal component loaded on the mesoporous carbon carrier; the mesoporous carbon carrier contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. The preparation method of the hydrogenation catalyst comprises the process of preparing a mesoporous carbon carrier and introducing a hydrogenation active metal into the mesoporous carbon carrier; the mesoporous carbon carrier preparation step comprises: mixing a carbon carrier precursor, a phosphorus source and a binder to obtain a mixed material, and heat-treating the mixed material under an oxygen-containing atmosphere. The preparation of the mesoporous carbon carrier in the present invention has the advantages of simple process flow and good environmental protection, and is suitable for industrial large-scale production of carbon carriers. Compared with the catalyst prepared by the prior art, the hydrogenation catalyst provided by the present invention has higher hydrogenation activity when used in the hydrogenation treatment of petroleum fractions and residual oils and the hydrogenation process of chemical raw materials and products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hydrogenation catalysts, and in particular to a hydrogenation catalyst containing a mesoporous carbon carrier, and a preparation method and application thereof. Background Art

[0002] The hydrogenation catalyst prepared by carbon carrier is beneficial to improve the hydrogenation activity of the catalyst because of the weak interaction between the carbon carrier and the metal component. In addition, the metal can be easily recovered from the spent catalyst by burning the carrier. Therefore, the application of carbon materials as carriers has always attracted much attention, especially mesoporous carbon material carriers.

[0003] At present, there are two main methods for synthesizing mesoporous carbon materials, hard template method and soft template method. 93120049.0 introduces a method for preparing activated carbon, especially a method for preparing activated carbon using asphalt as raw material. Its main technical feature is that the asphalt crushed into powder is mixed with an extrusion aid, a binder, etc. to form an activated carbon product; after anti-melting, carbonization and activation treatment, the activated carbon product can be obtained. 201710172091.0 provides a porous carbon and a preparation method thereof. The preparation method of the porous carbon includes the following steps: mixing coal liquefaction asphalt, tetraethyl orthosilicate, hydrochloric acid and an organic solvent to form a composite slurry; drying the composite slurry to obtain a composite; carbonizing the composite to obtain a carbonized product; and removing silicon dioxide from the carbonized product to obtain porous carbon. The step of removing silicon dioxide from the carbonized product includes: soaking the carbonized product in an aqueous NaOH solution or hydrofluoric acid for 12 to 24 hours to obtain the porous carbon.

[0004] The above preparation process is relatively complicated, and acid washing or alkali washing is required in the process, which will produce a certain amount of waste liquid; or an organic template is required, and the cost of raw materials is relatively high. Therefore, there is an urgent need for a technology with a simple process flow, low cost, and very suitable for large-scale industrial application to prepare mesoporous carbon materials, and then use the mesoporous carbon materials as carriers to prepare supported hydrogenation catalysts. Summary of the invention

[0005] The purpose of the present invention is to provide a hydrogenation catalyst using a mesoporous carbon material as a carrier, and to provide a preparation method of the hydrogenation catalyst and an application of the hydrogenation catalyst in hydrocarbon oil hydroprocessing. Specifically, the present invention includes the following contents.

[0006] The present invention provides a hydrogenation catalyst, which comprises a mesoporous carbon carrier and an active metal component loaded on the mesoporous carbon carrier, wherein the active metal component comprises at least one metal element of Group VIII and at least one metal element of Group VIB; the mesoporous carbon carrier contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus, and based on the total weight of the mesoporous carbon carrier, the carbon content is 80-90% by weight, the oxygen content is 2-6% by weight, the hydrogen content is 0.1-1% by weight, the sulfur content is 1-8% by weight, the nitrogen content is 0.5-3% by weight, and the phosphorus content is 0.5-10% by weight.

[0007] The present invention provides a method for preparing a hydrogenation catalyst, comprising the steps of preparing a mesoporous carbon carrier and introducing at least one metal element of Group VIII and at least one metal element of Group VIB into the mesoporous carbon carrier; the mesoporous carbon carrier contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus, and based on the total weight of the mesoporous carbon carrier, the carbon content is 80-90% by weight, the oxygen content is 2-6% by weight, the hydrogen content is 0.1-1% by weight, the sulfur content is 1-8% by weight, the nitrogen content is 0.5-3% by weight, and the phosphorus content is 0.5 ~10 wt %; wherein the preparation steps of the mesoporous carbon carrier include: (1) mixing a carbon carrier precursor, a phosphorus source, and a binder to obtain a mixture, wherein the carbon carrier precursor is asphalt powder and / or petroleum coke powder, and the phosphorus source is a phosphorus-containing compound, and the phosphorus-containing compound includes at least one of phosphoric acid, phosphates or phosphorus-containing organic compounds; (2) heat-treating the mixture in an oxygen-containing atmosphere; relative to 100 parts by weight of the asphalt powder and / or petroleum coke powder, the amount of the phosphorus source is 0.5 to 8 parts by weight, preferably 1 to 6 parts by weight, calculated as phosphorus pentoxide; the amount of the binder is 1 to 20 parts by weight, preferably 5 to 15 parts by weight.

[0008] The present invention also provides the use of any of the above-mentioned hydrogenation catalysts provided by the present invention or the hydrogenation catalysts prepared by any of the methods provided by the present invention in hydrocarbon oil hydrogenation treatment.

[0009] Compared with the catalyst prepared by the prior art, the catalyst provided by the present invention has higher hydrogenation activity when used in the hydrogenation treatment of petroleum fractions and residual oil and the hydrogenation process of chemical raw materials and products. DETAILED DESCRIPTION

[0010] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.

[0011] According to the hydrogenation catalyst provided by the present invention, the type and content of the hydrogenation active metal element are conventionally selected in the art. Generally, the metal element of Group VIII may be cobalt and / or nickel, and the metal element of Group VIB may be molybdenum and / or tungsten; preferably, based on the total amount of the catalyst, the content of the mesoporous carbon carrier is preferably 50-95% by weight, the content of the metal element of Group VIII calculated as oxide is 0.5-10% by weight, and the content of the metal element of Group VIB is 4-40% by weight; based on the total weight of the mesoporous carbon carrier, in terms of elements, the content of the carbon element is 82-88% by weight, the content of the oxygen element is 3-5% by weight, the content of the hydrogen element is 0.2-0.8% by weight, the content of the sulfur element is 2-6% by weight, the content of the nitrogen element is 1-2.5% by weight, and the content of the phosphorus element is 1-6% by weight.

[0012] The carbon carrier of the present invention is a mesoporous material with a larger pore size, some of which can reach more than 6nm. Generally, the pore size is 2 to 30nm, preferably 6 to 20nm. The present invention has no special requirements on the specific surface area and pore volume of the carbon carrier, such as the specific surface area can be 50 to 1200m 2 / g, preferably 100 to 1000 m 2 / g; the pore volume can be 0.3~1.3cm 3 / g, preferably 0.4 to 1.2 cm 3 / g.

[0013] According to the present invention, the hydrogenation catalyst preferably contains an organic auxiliary agent, which can be selected from at least one of an organic acid and / or its ammonium salt, an organic alcohol and a sugar compound, and the molar ratio of the organic auxiliary agent to the first active metal element can be (0.3-2):1. The organic auxiliary agent can make the active element component uniformly dispersed in the porous carbon carrier, thereby further improving the hydrogenation activity of the hydrogenation catalyst. Further preferably, the organic acid is selected from at least one of trans-1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid, aminotriacetic acid, citric acid, oxalic acid, acetic acid, formic acid, glyoxylic acid, glycolic acid, tartaric acid and malic acid; the organic alcohol is selected from at least one of glycerol, ethylene glycol, polyethylene glycol, trimethylolethane, pentaerythritol, xylitol and sorbitol; the sugar compound is selected from at least one of triose, tetrose, pentose, D-glucose, D-galactose, D-mannose, D-fructose and sucrose.

[0014] According to the present invention, the catalyst may also contain non-metallic additives for improving the catalytic performance, such as phosphorus additives, boron additives, etc. The phosphorus additives, in addition to the phosphorus contained in the carrier, may also be introduced together with the active metal and / or organic additives during the impregnation. The content of the additives is conventionally selected, for example, based on the weight of the catalyst and calculated as P2O5, the phosphorus content is 0.5-10% by weight, preferably 1-8% by weight, and the boron content calculated as B2O3 is 0.5-10% by weight, preferably 1-8% by weight.

[0015] According to the method for preparing a hydrogenation catalyst provided by the present invention, preferably, based on the total weight of the mesoporous carbon carrier, in terms of elements, the content of the carbon element is 82-88% by weight, the content of the oxygen element is 3-5% by weight, the content of the hydrogen element is 0.2-0.8% by weight, the content of the sulfur element is 2-6% by weight, the content of the nitrogen element is 1-2.5% by weight, and the content of the phosphorus element is 1-6% by weight. Preferably, the metal element of Group VIII is cobalt and / or nickel, and the metal element of Group VIB is molybdenum and / or tungsten. The amount of each component is such that based on the total amount of the catalyst, the content of the mesoporous carbon carrier is 59-94% by weight, the content of the metal element of Group VIII in terms of oxide is 1-6% by weight, and the content of the metal element of Group VIB is 5-35% by weight. According to needs, non-metallic additives, such as additives phosphorus, boron, etc., can be introduced during the preparation of the catalyst. Non-metallic additives can be introduced together with active metals and / or organic additives. There is no special requirement for the amount of non-metallic additives introduced. For example, based on the total amount of the catalyst, the phosphorus content is 0.5-10% by weight, preferably 1-8% by weight, calculated as P2O5, and the boron content is 0.5-10% by weight, preferably 1-8% by weight, calculated as B2O3.

[0016] According to the present invention, the carbon carrier precursors may be asphalt powder and / or petroleum coke powder, or they may be used as precursors after being subjected to oxygen heat treatment (oxygen heat treatment). Specifically, petroleum coke is a product obtained by thermal cracking and conversion of heavy oil obtained by crude oil distillation. Asphalt powder oxygen heat product or petroleum coke powder oxygen heat product refers to the product obtained after asphalt powder or petroleum coke powder is subjected to oxygen heat treatment in an oxygen-containing atmosphere. Among them, the conditions for oxygen heat treatment may include: an oxygen-containing gas flow rate of 1 to 80 liters / hour, a heating rate of 0.1 to 10°C / minute, an oxygen heat treatment temperature of 120 to 450°C, and an oxygen heat treatment time of 1 to 48 hours.

[0017] The phosphorus source can be converted into phosphorus pentoxide during the heat treatment process, which may contain a small amount of other impurity elements, such as a small amount of metal elements, in addition to C, H, O and P. The phosphate may be, for example, potassium, sodium or ammonium phosphate.

[0018] In the carbon carrier preparation method provided by the present invention, a carbon carrier precursor and a phosphorus source are evenly mixed under the action of a binder, and then heat-treated to obtain a mesoporous carbon carrier. Since the carbon carrier precursor and the phosphorus source are both cheap raw materials, and no high-cost organic template is required in the preparation process, the method of the present invention has the advantage of low cost; moreover, the method does not involve the dissolution process of the template, and successfully avoids the use of a solvent with poor environmental protection to dissolve the template. Therefore, the method of the present invention also has the advantages of simple process flow and good environmental protection, and is suitable for industrial large-scale production of carbon carriers.

[0019] According to the present invention, the amount of carbon in the precursor, phosphorus source and adhesive can vary within a certain range. For example, relative to 100 parts by weight of the carbon carrier precursor, the amount of the phosphorus source can be 0.5 to 8 parts by weight, preferably 1 to 6 parts by weight, calculated as phosphorus pentoxide; the amount of the adhesive can be 1 to 20 parts by weight, preferably 5 to 15 parts by weight.

[0020] In order to make the materials mix faster and better, preferably, the carbon carrier precursor and the phosphorus source can have a smaller particle size, for example, the particle size of the carbon carrier precursor can be 1 to 1000 μm, preferably 1 to 250 μm. In order to further improve the uniformity of mixing, when mixing the carbon carrier precursor, the phosphorus source and the binder, the binder can be impregnated with an aqueous solution of the phosphorus source, and then the carbon carrier precursor can be added and stirred to mix.

[0021] According to the present invention, the binder may include at least one of cellulose ether, starch or enol polymer, preferably cellulose ether, more preferably at least one of methyl cellulose, hydroxyethyl methyl cellulose or hydroxypropyl methyl cellulose.

[0022] According to the present invention, the asphalt powder can be selected within a certain range. For example, the asphalt powder can include petroleum asphalt powder and / or coal asphalt powder. The asphalt powder can contain polycyclic aromatic hydrocarbons. Based on the total weight of the asphalt powder, the content of the polycyclic aromatic hydrocarbons can be 70 to 100 weight %, preferably 85 to 100 weight %.

[0023] According to the present invention, the heat treatment of the mixed material in an oxygen-containing atmosphere to obtain the mesoporous carbon carrier may include: in an oxygen-containing atmosphere, the temperature of the mixed material is raised from room temperature to 120-450°C at a heating rate of 0.1-10°C / min, and a first heat treatment is performed for 0.1-48 hours to obtain an intermediate product; in an oxygen-containing atmosphere, the temperature of the intermediate product is raised to 700-1000°C at a heating rate of 0.1-10°C / min, and a second heat treatment is performed for 0.1-12 hours to obtain the mesoporous carbon carrier. Wherein, the oxygen-containing atmosphere contains an oxygen-containing gas, or a mixed gas of an oxygen-containing gas and an inert gas, wherein the oxygen-containing gas includes at least one of oxygen, carbon dioxide and carbon monoxide; and the inert gas includes at least one of nitrogen, argon and helium. Further, the flow rate of the oxygen-containing gas flow during the first heat treatment may be 0.1-80 liters / hour, and the flow rate of the oxygen-containing gas flow during the second heat treatment may be 0.1-80 liters / hour.

[0024] In the present invention, any means in the prior art can be used to load the hydrogenation active metal onto the carbon carrier, preferably an impregnation method, specifically, the hydrogenation active metal is configured into an aqueous solution, and then the carbon carrier is impregnated, and the hydrogenation catalyst is obtained after drying. The amount of each component is used so that the content of the carbon carrier and the active metal in the finally obtained hydrogenation catalyst meets the requirements of the present invention for each component. According to the method for preparing a hydrogenation catalyst provided by the present invention, when the catalyst contains an organic auxiliary agent, the preparation method correspondingly includes the step of introducing the organic auxiliary agent. The organic auxiliary agent can be introduced into the carrier at the same time as the hydrogenation active component, or it can be introduced before or after the introduction of the hydrogenation active metal. When a separate introduction scheme is adopted, appropriate drying treatment can be performed after each introduction. Preferably, the organic auxiliary agent is selected from at least one of organic acids and / or ammonium salts thereof, organic alcohols and sugar compounds, and the molar ratio of the organic auxiliary agent to the Group VIII metal element is (0.3-2):1; the organic acid is selected from at least one of trans-1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid, aminotriacetic acid, citric acid, oxalic acid, acetic acid, formic acid, glyoxylic acid, glycolic acid, tartaric acid and malic acid; the organic alcohol is selected from at least one of glycerol, ethylene glycol, polyethylene glycol, trimethylolethane, pentaerythritol, xylitol and sorbitol; the sugar compound is selected from at least one of trioses, tetroses, pentoses, D-glucose, D-galactose, D-mannose, D-fructose and sucrose.

[0025] Finally, according to the application of the catalyst provided by the present invention in hydrocarbon oil hydroprocessing, the hydroprocessing catalyst should generally be first sulfurized and then hydroprocessed. Specifically, the hydrocarbon oil feedstock can be contacted with the catalyst of the present invention or the catalyst prepared by the method of the present invention under hydroprocessing conditions, and the hydroprocessing conditions are conventional conditions. For example: pressure 0.2-14MPa, hydrogen-to-oil volume ratio 50-500:1, volume space velocity 1-8h -1 , temperature is 200-400℃, time is 2-12 hours.

[0026] The present disclosure is further described below by way of examples, but the present disclosure is not limited thereby. The raw materials, reagents, instruments and equipment involved in the examples of the present disclosure can all be purchased unless otherwise specified.

[0027] Petroleum coke powder oxygen thermal product SYJ-450 powder: petroleum coke is placed in a muffle furnace, air is passed through and the flow rate is controlled at 80 liters / hour, the temperature of the mixture is raised to 450°C at a heating rate of 5°C / min, and maintained at 450°C for 4 hours. The obtained product is crushed to obtain SYJ-450 powder.

[0028] Petroleum coke powder oxygen thermal product SYJ-400 powder: petroleum coke is placed in a muffle furnace, air is passed through and the flow rate is controlled at 80 liters / hour, the temperature of the mixture is raised to 400°C at a heating rate of 5°C / min, and maintained at 400°C for 4 hours. The obtained product is crushed to obtain SYJ-400 powder.

[0029] Petroleum coke powder oxygen thermal product SYJ-350 powder: petroleum coke is placed in a muffle furnace, air is passed through and the flow rate is controlled at 80 liters / hour, the temperature of the mixture is raised to 350°C at a heating rate of 5°C / min, and maintained at a constant temperature of 350°C for 4 hours. The obtained product is crushed to obtain SYJ-350 powder.

[0030] Asphalt powder oxygen thermal product LQ-350 powder: Place the asphalt in a muffle furnace, pass air and control the flow rate to 80 liters / hour, raise the temperature of the mixture to 350℃ at a heating rate of 5℃ / min, and maintain a constant temperature of 350℃ for 4 hours. The obtained product is crushed to obtain LQ-350 powder.

[0031] Asphalt powder oxygen thermal product LQ-300 powder: Place the asphalt in a muffle furnace, pass air and control the flow rate to 80 liters / hour, raise the temperature of the mixture to 300°C at a heating rate of 5°C / min, and maintain a constant temperature of 300°C for 4 hours. The obtained product is crushed to obtain LQ-300 powder.

[0032] Preparation Example 1

[0033] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred, and allowed to stand for 2 hours, then 500 g of asphalt powder was added, stirred and mixed evenly to obtain a mixture. 200 g of the above mixture was placed in a closed tube furnace, air was passed through and the flow rate was controlled to 40 liters / hour, the temperature of the mixture was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 360°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain a mesoporous carbon carrier S1.

[0034] In this preparation example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (phosphoric acid) used is 3.69 parts by weight, and the amount of binder (methyl cellulose) used is 10 parts by weight, calculated as phosphorus pentoxide.

[0035] S1 contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. Based on the total weight of the mesoporous carbon carrier S1, the carbon content is 82.16% by weight, the oxygen content is 4.47% by weight, the hydrogen content is 0.49% by weight, the sulfur content is 6.00% by weight, the nitrogen content is 1.47% by weight and the phosphorus content is 5.41% by weight.

[0036] Preparation Example 2

[0037] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 10 g of phosphoric acid (mass fraction 85%), stirred, and allowed to stand for 2 hours, then 500 g of asphalt powder was added, stirred and mixed to obtain a mixture. 200 g of the above mixture was placed in a closed tube furnace, air was passed through and the flow rate was controlled to 40 liters / hour, the temperature of the mixture was raised to 240°C at a heating rate of 5°C / minute, and maintained at 240°C for 18 hours, and then raised to 340°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to 40 liters / hour, the temperature of the intermediate product was raised to 950°C at a heating rate of 5°C / minute, and maintained at 950°C for 4 hours to obtain a mesoporous carbon carrier S2.

[0038] In this preparation example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (phosphoric acid) used is 2 parts by weight, and the amount of binder (methyl cellulose) used is 10 parts by weight, calculated as phosphorus pentoxide.

[0039] S2 contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. Based on the total weight of the mesoporous carbon carrier S2, the carbon content is 86.58% by weight, the oxygen content is 3.78% by weight, the hydrogen content is 0.52% by weight, the sulfur content is 5.57% by weight, the nitrogen content is 1.62% by weight and the phosphorus content is 1.93% by weight.

[0040] Preparation Example 3

[0041] A mixture of 60 g of methyl cellulose, 20 g of hydroxyethyl methyl cellulose and 20 g of hydroxypropyl methyl cellulose was impregnated with 200 ml of an aqueous solution containing 21 g of phosphoric acid (mass fraction 85%), stirred evenly, and then allowed to stand for 2 hours, and then 500 g of asphalt powder was added, stirred and mixed to obtain a mixture. 200 g of the above mixture was placed in a closed tubular furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixture was raised to 350°C at a heating rate of 5°C / minute, and maintained at 350°C for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 6 hours to obtain a mesoporous carbon carrier S3.

[0042] In this preparation example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (phosphoric acid) used is 4.2 parts by weight, and the amount of binder (methyl cellulose+hydroxyethyl methyl cellulose+hydroxypropyl methyl cellulose) used is 10 parts by weight, calculated as phosphorus pentoxide.

[0043] S3 contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. Based on the total weight of the mesoporous carbon carrier S3, the carbon content is 87.72% by weight, the oxygen content is 2.81% by weight, the hydrogen content is 0.37% by weight, the sulfur content is 4.51% by weight, the nitrogen content is 1.52% by weight and the phosphorus content is 3.07% by weight.

[0044] Preparation Example 4

[0045] The carbon carrier S4 was prepared according to the method of Preparation Example 1, except that in this preparation example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (phosphoric acid) used was 0.5 parts by weight, and the amount of binder (methyl cellulose) used was 1 part by weight, calculated as phosphorus pentoxide.

[0046] Preparation Example 5

[0047] The carbon carrier S5 was prepared according to the method of Preparation Example 1, except that in this preparation example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (sodium phosphate) used was 8 parts by weight, and the amount of binder (starch) used was 20 parts by weight, calculated as phosphorus pentoxide.

[0048] Preparation Example 6

[0049] The carbon carrier S6 was prepared according to the method of Preparation Example 1, except that in this Preparation Example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (potassium phosphate) used was 1 part by weight, and the amount of binder (enol polymer) used was 5 parts by weight, calculated as phosphorus pentoxide.

[0050] Preparation Example 7

[0051] The carbon carrier S7 was prepared according to the method of Preparation Example 1, except that in this preparation example, relative to 100 parts by weight of asphalt powder, the amount of phosphorus source (ammonium phosphate) used was 6 parts by weight, and the amount of binder (methyl cellulose) used was 15 parts by weight, calculated as phosphorus pentoxide.

[0052] Preparation Example 8

[0053] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred, and allowed to stand for 2 hours. Then, 200 g of petroleum coke powder, 100 g of asphalt powder, 20 g of SYJ-450 powder, 50 g of SYJ-400 powder, 30 g of SYJ-350 powder, 50 g of LQ-350 powder, and 50 g of LQ-300 powder were added, and the mixture was stirred and mixed evenly to obtain a mixed material. Take 200 grams of the above-mentioned mixed material and place it in a closed tubular furnace, let air flow and control the flow rate to 40 L / hour, raise the temperature of the mixed material to 120°C at a heating rate of 5°C / min, and maintain a constant temperature of 120°C for heat treatment for 32 hours, then raise the temperature to 400°C at 1°C / min and maintain the constant temperature for 4 hours to obtain an intermediate product; then, switch the air to carbon dioxide gas and control the flow rate to 40 L / hour, raise the temperature of the intermediate product to 960°C at a heating rate of 5°C / min, and maintain a constant temperature of 960°C for heat treatment for 4 hours to obtain the mesoporous carbon support S8.

[0054] In this preparation example, relative to 100 parts by weight of the carbon source, the amount of the phosphorus source (phosphoric acid) is 3.69 parts by weight, and the amount of the binder (methyl cellulose) is 10 parts by weight, calculated as phosphorus pentoxide. S8 contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. Based on the total weight of the mesoporous carbon carrier S8, the carbon content is 87.59% by weight, the oxygen content is 2.51% by weight, the hydrogen content is 0.37% by weight, the sulfur content is 4.09% by weight, the nitrogen content is 2.28% by weight, and the phosphorus content is 3.16% by weight.

[0055] Preparation Example 9

[0056] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 35 g of phosphoric acid (mass fraction 85%), stirred, and allowed to stand for 2 hours, then 400 g of asphalt powder, 10 g of SYJ-450 powder, 80 g of SYJ-400 powder, and 10 g of SYJ-350 powder were added, and the mixture was stirred and mixed evenly to obtain a mixed material. 200 g of the above mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 350°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 940°C at a heating rate of 5°C / minute, and maintained at 940°C for 4 hours to obtain a mesoporous carbon carrier S9.

[0057] In this preparation example, relative to 100 parts by weight of the carbon source, the amount of the phosphorus source (phosphoric acid) is 4.31 parts by weight, and the amount of the binder (methyl cellulose) is 10 parts by weight, calculated as phosphorus pentoxide. S9 contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. Based on the total weight of the mesoporous carbon carrier S9, the carbon content is 87.36% by weight, the oxygen content is 2.40% by weight, the hydrogen content is 0.40% by weight, the sulfur content is 5.03% by weight, the nitrogen content is 1.68% by weight, and the phosphorus content is 3.13% by weight.

[0058] Preparation Example 10

[0059] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred, and allowed to stand for 2 hours, then 500 g of petroleum coke powder was added, stirred and mixed evenly to obtain a mixed material. 200 g of the above mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 400°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain a mesoporous carbon carrier S10.

[0060] In this preparation example, relative to 100 parts by weight of petroleum coke powder, the amount of phosphorus source (phosphoric acid) is 3.69 parts by weight, and the amount of binder (methyl cellulose) is 10 parts by weight, calculated as phosphorus pentoxide. S10 contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus. Based on the total weight of the mesoporous carbon carrier S10, the carbon content is 87.91% by weight, the oxygen content is 2.29% by weight, the hydrogen content is 0.33% by weight, the sulfur content is 4.35% by weight, the nitrogen content is 2.36% by weight, and the phosphorus content is 2.76% by weight.

[0061] Preparation Comparative Example 1

[0062] 50 g of methyl cellulose was soaked in 200 ml of water, stirred evenly, and allowed to stand for 2 hours, then 500 g of asphalt powder was added, stirred and mixed to obtain a mixture. 200 g of the above mixture was placed in a closed tube furnace, air was passed through and the flow rate was controlled to 40 liters / hour, the temperature of the mixture was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 360°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain the product DT-1.

[0063] Preparation Comparative Example 2

[0064] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred evenly, and then allowed to stand for 2 hours, and then 500 g of asphalt powder was added, stirred and mixed to obtain a mixed material. 200 g of the above mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 360°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to nitrogen and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain a product DT-2.

[0065] Preparation Comparative Example 3

[0066] 500 g of asphalt powder was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred and mixed to obtain a mixed material. 200 g of the mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 360°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain the product DT-3.

[0067] Preparation Comparative Example 4

[0068] 50 g of methyl cellulose was soaked in 200 ml of water, stirred, and allowed to stand for 2 hours, then 500 g of petroleum coke powder was added, stirred and mixed to obtain a mixed material. 200 g of the mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 400°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain the product DT-4.

[0069] Preparation Comparative Example 5

[0070] 50 g of methyl cellulose was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred, and allowed to stand for 2 hours, then 500 g of petroleum coke powder was added, stirred and mixed to obtain a mixed material. 200 g of the above mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 400°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to nitrogen and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain a product DT-5.

[0071] Preparation Comparative Example 6

[0072] 500 g of petroleum coke powder was impregnated with 200 ml of an aqueous solution containing 30 g of phosphoric acid (mass fraction 85%), stirred and mixed to obtain a mixed material. 200 g of the mixed material was placed in a closed tube furnace, air was passed through and the flow rate was controlled to be 40 liters / hour, the temperature of the mixed material was raised to 120°C at a heating rate of 5°C / minute, and maintained at 120°C for 32 hours, and then raised to 400°C at 1°C / min for 4 hours to obtain an intermediate product; then, the air was switched to carbon dioxide gas and the flow rate was controlled to be 40 liters / hour, the temperature of the intermediate product was raised to 960°C at a heating rate of 5°C / minute, and maintained at 960°C for 4 hours to obtain the product DT-6.

[0073] Test Case

[0074] The pore structure of each product prepared in Preparation Examples 1-10 and Comparative Preparation Examples 1-6 was measured, and the measurement results are shown in Table 1.

[0075] Table 1

[0076] product Pore ​​diameter(nm) <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Pore volume (cm 3 / g)]]> S1 10 386 0.51 S2 8 280 0.52 S3 11 285 0.51 S4 6 156 0.32 S5 19 259 0.50 S6 7 228 0.45 S7 17 267 0.53 S8 15 488 0.68 S9 12 353 0.45 S10 16 369 0.65 DT-1 2 6 0.01 DT-2 2 42 0.02 DT-3 3 15 0.02 DT-4 2 85 0.05 DT-5 2 1 0.01 DT-6 3 72 0.11

[0077] It can be seen from Table 1 that the mesoporous carbon carrier obtained in the preparation example has a larger pore size (above 6 nm). The carbon carriers obtained in the preparation example and the comparative example are used to prepare hydrogenation catalysts.

[0078] Examples 1-10

[0079] 200 g of the S1-S10 carbon carrier obtained by the above method was impregnated with 170 mL of an aqueous solution containing 3.98 g of phosphoric acid (85%), 42.12 g of molybdenum trioxide, 17.21 g of basic nickel carbonate (NiO content 51%), 22.56 g of citric acid, 2.29 g of ethylene glycol and 3.62 g of propylene glycol. After stirring evenly, the mixture was allowed to stand for 2 h and dried at 120°C for 4 h to obtain catalyst C1-10.

[0080] Comparative Examples 1-6

[0081] The contrast agent was prepared in the same manner as in the examples, the only difference being that the carbon carriers were the carriers DT-1 to DT-6 obtained in comparative preparation examples 1-6, and the contrast agents obtained were denoted as DC1 to DC6.

[0082] Catalyst performance evaluation

[0083] The hydrodesulfurization activities of catalysts C1-C10 and DC1-DC6 were evaluated using straight-run kerosene (total sulfur 869 μg / g) as the reaction raw material.

[0084] The evaluation device is a fixed bed hydrogenation reactor, the catalyst particle size is 20-30 mesh, and the catalyst dosage is 30ml. Hydrogen is passed once. Before the reaction, the catalyst is first pre-sulfurized, and the sulfurized oil is straight-run kerosene containing 2% CS2. The sulfurization conditions are: pressure 1.6MPa, hydrogen oil volume ratio 100:1, volume space velocity 4h -1 , temperature 300℃, time 4 hours. After sulfurization, the feed was switched to straight-run kerosene. The reaction conditions included: reaction temperature 240℃, volume space velocity 4h -1 , reaction pressure 1.6 MPa, hydrogen to oil ratio 100: 1. After 6 days of reaction at 240°C, samples were taken for analysis, and the results are listed in Table 2.

[0085] Table 2

[0086]

[0087]

[0088] Compared with the comparative agent, the catalyst provided by the present invention exhibits higher hydrodesulfurization activity.

Claims

1. A hydrogenation catalyst, comprising a mesoporous carbon support and an active metal component supported on the mesoporous carbon support, wherein the active metal component comprises at least one metal element of Group VIII and at least one metal element of Group VIB; the mesoporous carbon support contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus, and based on the total weight of the mesoporous carbon support, the carbon content is 80-90% by weight, the oxygen content is 2-6% by weight, the hydrogen content is 0.1-1% by weight, the sulfur content is 1-8% by weight, the nitrogen content is 0.5-3% by weight, and the phosphorus content is 0.5-10% by weight; in, The specific surface area of ​​the mesoporous carbon carrier is 50 to 1200 m 2 / g; pore volume is 0.3~1.3 cm 3 / g; the pore size is 2 to 30 nm.

2. The hydrogenation catalyst according to claim 1, wherein The VIII group metal element is cobalt and / or nickel, the VIB group metal element is molybdenum and / or tungsten. Based on the total amount of catalyst, the content of the mesoporous carbon carrier is 50-95% by weight, the content of the VIII group metal element in terms of oxide is 0.5-10% by weight, and the content of the VIB group metal element is 4-40% by weight; based on the total weight of the mesoporous carbon carrier, in terms of elements, the content of the carbon element is 82-88% by weight, the content of the oxygen element is 3-5% by weight, the content of the hydrogen element is 0.2-0.8% by weight, the content of the sulfur element is 2-6% by weight, the content of the nitrogen element is 1-2.5% by weight, and the content of the phosphorus element is 1-6% by weight.

3. The hydrogenation catalyst according to claim 1, wherein The specific surface area of ​​the mesoporous carbon carrier is 100 to 1000 m 2 / g; pore volume is 0.4~1.2 cm 3 / g; the pore size is 6 to 20 nm.

4. The hydrogenation catalyst according to claim 1, wherein The hydrogenation catalyst contains an organic auxiliary agent, which is selected from at least one of an organic acid and / or its ammonium salt, an organic alcohol and a sugar compound, and the molar ratio of the organic auxiliary agent to the Group VIII metal element is (0.3-2):1; the organic acid is selected from at least one of trans-1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid, aminotriacetic acid, citric acid, oxalic acid, acetic acid, formic acid, glyoxylic acid, glycolic acid, tartaric acid and malic acid; the organic alcohol is selected from at least one of glycerol, ethylene glycol, polyethylene glycol, trimethylolethane, pentaerythritol, xylitol and sorbitol; the sugar compound is selected from at least one of triose, tetrose, pentose, D-glucose, D-galactose, D-mannose, D-fructose and sucrose.

5. A method for preparing a hydrogenation catalyst, comprising the process of preparing a mesoporous carbon carrier and introducing at least one Group VIII metal element and at least one Group VIB metal element into the mesoporous carbon carrier; the mesoporous carbon carrier contains carbon, oxygen, hydrogen, sulfur, nitrogen and phosphorus, and based on the total weight of the mesoporous carbon carrier, the carbon content is 80-90% by weight, the oxygen content is 2-6% by weight, the hydrogen content is 0.1-1% by weight, the sulfur content is 1-8% by weight, the nitrogen content is 0.5-3% by weight, and the phosphorus content is 0.5-10% by weight; the steps of preparing the mesoporous carbon carrier include: (1) mixing a carbon carrier precursor, a phosphorus source, and a binder to obtain a mixed material, wherein the carbon carrier precursor is asphalt powder and / or petroleum coke powder, the phosphorus source is a phosphorus-containing compound, and the phosphorus-containing compound includes at least one of phosphoric acid, phosphate, or a phosphorus-containing organic compound; (2) heat-treating the mixed material in an oxygen-containing atmosphere; Relative to 100 parts by weight of the asphalt powder and / or petroleum coke powder, the amount of the phosphorus source is 0.5 to 8 parts by weight in terms of phosphorus pentoxide; the amount of the binder is 1 to 20 parts by weight.

6. The method according to claim 5, characterized in that Relative to 100 parts by weight of the asphalt powder and / or petroleum coke powder, the amount of the phosphorus source is 1 to 6 parts by weight in terms of phosphorus pentoxide; the amount of the binder is 5 to 15 parts by weight.

7. The method according to claim 5, characterized in that The particle size of the asphalt powder and / or petroleum coke powder is 1 to 1000 μm.

8. The method according to claim 7, characterized in that The particle size of the asphalt powder and / or petroleum coke powder is 1 to 250 μm.

9. The method according to claim 5, wherein: The binder includes at least one of cellulose ether, starch or enol polymer.

10. The method according to claim 9, wherein: The binder is at least one of methyl cellulose, hydroxyethyl methyl cellulose or hydroxypropyl methyl cellulose.

11. The method according to claim 5, wherein: The asphalt powder includes petroleum asphalt powder and / or coal asphalt powder. The asphalt powder contains polycyclic aromatic hydrocarbons. Based on the total weight of the asphalt powder, the content of the polycyclic aromatic hydrocarbons is 70-100% by weight.

12. The method according to claim 11, wherein: Based on the total weight of the asphalt powder, the content of the polycyclic aromatic hydrocarbons is 85 to 100 weight %.

13. The method according to any one of claims 5 to 12, wherein: The conditions for heat treating the mixed material in an oxygen-containing atmosphere include: In an oxygen-containing atmosphere, the temperature of the mixed material is raised from room temperature to 120-450° C. at a heating rate of 0.1-10° C. / min, and a first heat treatment is performed for 0.1-48 hours to obtain an intermediate product; In an oxygen-containing atmosphere, the temperature of the intermediate product is raised to 700-1000° C. at a heating rate of 0.1-10° C. / min, and a second heat treatment is performed for 0.1-12 hours to obtain the mesoporous carbon support.

14. The method according to claim 13, wherein: The oxygen-containing atmosphere contains an oxygen-containing gas, or a mixed gas of an oxygen-containing gas and an inert gas, wherein the oxygen-containing gas includes at least one of oxygen, carbon dioxide and carbon monoxide, and the inert gas includes at least one of nitrogen, argon and helium.

15. The method according to claim 5, wherein: The method also includes the step of introducing an organic auxiliary agent on the mesoporous carbon carrier, wherein the organic auxiliary agent is introduced simultaneously with the active metal or introduced successively, the organic auxiliary agent is selected from at least one of organic acids and / or ammonium salts thereof, organic alcohols and sugar compounds, and the molar ratio of the organic auxiliary agent to the metal element of Group VIII is (0.3-2):1; the organic acid is selected from at least one of trans-1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid, aminotriacetic acid, citric acid, oxalic acid, acetic acid, formic acid, glyoxylic acid, glycolic acid, tartaric acid and malic acid; the organic alcohol is selected from at least one of glycerol, ethylene glycol, polyethylene glycol, trimethylolethane, pentaerythritol, xylitol and sorbitol; the sugar compound is selected from at least one of trioses, tetroses, pentoses, D-glucose, D-galactose, D-mannose, D-fructose and sucrose.

16. Use of the hydrogenation catalyst according to any one of claims 1 to 4 or the catalyst prepared by the method according to any one of claims 5 to 15 in hydrocarbon oil hydroprocessing.