Molecular sieve coating slurry for monolithic catalyst and method thereof
By using a dispersant combination of polyacrylamide, hydroxymethyl cellulose and acidic silica sol, a stable and uniform molecular sieve coating slurry is prepared, which solves the problems of molecular sieve catalyst slurry settlement and viscosity instability in the existing technology, and improves efficiency The catalytic performance and loading rate simplify the process and enhance the NOx conversion efficiency.
Patent Information
- Application Number
- CN202211627505.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-16
AI Technical Summary
The preparation method of honeycomb carrier catalyst loaded with molecular sieve components in the prior art has problems such as rapid slurry settling, unstable viscosity, easy pore blocking, low adhesion, complex process and narrow window, which affects the catalytic performance.
Polyacrylamide, hydroxymethylcellulose and acidic silica sol are used as dispersants, and the molecular sieve coating slurry is prepared through planetary ball mill dispersion to avoid agglomeration and improve the stability and uniformity of the slurry. Acidic silica sol is used as the binder. , reducing process steps and operational difficulty.
The stability and uniformity of the molecular sieve coating slurry are achieved, the loading rate and catalytic performance of the catalyst are improved, the shedding rate is reduced, the process flow is simplified, the operating window is broadened, and the NOx conversion efficiency is enhanced.
Smart Images

Figure BDA0004004229570000071 
Figure BDA0004004229570000091
Abstract
Description
Technical Field
[0001] The invention relates to a molecular sieve catalyst, in particular to a molecular sieve coating slurry for an integral catalyst and a method thereof. Background Art
[0002] With the increase in the number of cars, the contribution of pollutant emissions in automobile exhaust to air pollution continues to increase. Diesel engine NOx emissions are more serious than gasoline engines, and diesel engine exhaust treatment has become one of the problems that need to be solved urgently. Urea-selective catalystic reduction (Urea-SCR) is one of the most effective ways to solve diesel engine NOx pollution. The core of this technology lies in the research of catalysts. In recent years, honeycomb carrier catalysts loaded with molecular sieve components have begun to be used in the fields of industrial catalysis and environmental catalysis. This catalyst usually includes a honeycomb carrier and a molecular sieve component (molecular sieve or a composition containing molecular sieve) loading layer, wherein the honeycomb carrier is a whole block that has been formed and prepared, and has long, straight channels inside, and the molecular sieve components are loaded on the inner and / or outer walls of the channels.
[0003] The methods reported in the prior art for preparing honeycomb carrier catalysts loaded with molecular sieve components include in-situ synthesis. The in-situ synthesis method is to directly synthesize the molecular sieve coating on the carrier so that the molecular sieve can be combined with the carrier in the form of chemical bonds, thereby firmly growing on the carrier. However, the in-situ synthesis method cannot well control the loading amount and thickness of the coating, and the prepared molecular sieve monolithic catalyst has unstable quality, is difficult to replicate, and is not easy to industrialize. The commonly used method in the prior art is to load the molecular sieve component on the honeycomb carrier by coating. For example, for the currently more widely used honeycomb carrier catalysts loaded with Cu-type molecular sieves, the preparation method is mostly to coat the prepared Cu / SAPO-34, Cu / SSZ-13, and Cu / ZSM-5 catalysts on the surface of the cordierite honeycomb ceramic carrier through a binder.
[0004] Chinese patent document CN 107597178A provides a method for an integral molecular sieve type SCR catalyst, and the specific steps are as follows: (1) grinding the molecular sieve catalyst and passing it through a 40-mesh sieve; (2) dispersing the binder and the catalyst in deionized water in a mass ratio of 1: (2-5); (3) adjusting the pH to be acidic; (4) ball milling to prepare a slurry; (5) immersing the carrier in the slurry, taking it out, blowing off the residual liquid, aging, drying and then calcining to obtain a denitration integral catalyst. The method has a long stirring time and the resulting slurry has poor stability. If the stirring is stopped, the molecular sieve will quickly settle and affect the coating result, causing problems such as pore blockage and uneven coating. These factors will affect the loading rate and stability of the molecular sieve catalyst, and thus affect the catalytic performance.
[0005] Many scholars at home and abroad have tried to solve the above problems by adding dispersants or changing binders. Although the improved coating catalyst has improved the catalyst performance or coating strength to a certain extent, the molecular sieve slurry still generally has the problem of rapid sedimentation. At the same time, when using aluminum sol as a binder, the slurry needs to go through an aging process. These improvements also increase the difficulty of operation, not only narrowing the process window, but also complicating the preparation process of the catalyst. Therefore, there is a need for a coating slurry preparation method that has a simple process, good catalytic activity, does not require aging, and can increase the stability of the coating slurry. Summary of the invention
[0006] The present invention aims to solve at least one of the above technical problems.
[0007] The present invention provides a molecular sieve coating slurry for an integral catalyst and a preparation method thereof. The preparation method is designed to solve the problems of the existing molecular sieve catalyst slurry, such as fast sedimentation, unstable viscosity, easy pore blocking, low adhesion, long and complicated process and narrow window.
[0008] A molecular sieve coating slurry comprises: molecular sieve, polyacrylamide, hydroxymethyl cellulose, acidic silica sol and water; wherein, in the molecular sieve coating slurry, the mass ratio of the molecular sieve to water is 1:(1-2.3), and the mass ratio of the acidic silica sol to water is 1:(3-6).
[0009] The inventors have found that the combined action of polyacrylamide, hydroxymethyl cellulose and acidic silica sol can effectively prevent the molecular sieve coating slurry from agglomerating; the use of polyacrylamide and hydroxymethyl cellulose, two organic dispersants, prevents the slurry from agglomerating due to uneven dispersion of the dispersant in water.
[0010] According to an embodiment of the present invention, in the molecular sieve coating slurry, the mass ratio of the acidic silica sol to water is based on the dry weight of the acidic silica sol (eg, acidic silica sol dry powder).
[0011] According to an embodiment of the present invention, the average particle size of the acidic silica sol is 10-40 nm.
[0012] According to an embodiment of the present invention, in the molecular sieve coating slurry, the mass ratio of the molecular sieve to water is 1:1, 1:1.25, 1:1.5, 1:2, or 1:2.3.
[0013] According to an embodiment of the present invention, in the molecular sieve coating slurry, the mass ratio of acidic silica sol to water is 1:3, 1:4, 1:5 or 1:6.
[0014] According to an embodiment of the present invention, in the molecular sieve coating slurry, the mass ratio of molecular sieve to polyacrylamide is (700-800):1, which can be optionally 700:1, 750:1 or 800:1; the mass ratio of molecular sieve to hydroxymethyl cellulose is (700-800):1, which can be optionally 700:1, 750:1 or 800:1.
[0015] According to an embodiment of the present invention, in the molecular sieve coating slurry, the mass ratio of polyacrylamide to hydroxymethyl cellulose is 1:(0.8-1.2), which can be optionally 1:0.8, 1:1 or 1:1.2.
[0016] According to an embodiment of the present invention, the molecular sieve is SSZ-13 or SSZ-39; alternatively, the molecular sieve is Cu-SSZ-13 or Cu-SSZ-39, wherein the loading amount of Cu is 2%-4%.
[0017] According to an embodiment of the present invention, the water is deionized water.
[0018] According to an embodiment of the present invention, the pH of the molecular sieve coating slurry is 3-4.
[0019] According to an embodiment of the present invention, the potential value of the molecular sieve coating slurry is 54-58 mV.
[0020] According to an embodiment of the present invention, the molecular sieve coating slurry does not contain aluminum sol.
[0021] The present invention also provides a method for preparing the above-mentioned molecular sieve coating slurry, comprising: first mixing molecular sieve, polyacrylamide and hydroxymethyl cellulose, then mixing with water and acidic silica sol, and performing ball milling dispersion to prepare molecular sieve coating slurry.
[0022] The present invention selects two organic dispersants, polyacrylamide and hydroxymethyl cellulose, which play a key role in the slurry state, and adopts a method of first mixing the molecular sieve powder with the dispersant to avoid agglomeration of the slurry caused by uneven dispersion of the dispersant in water.
[0023] According to the present invention, the method for preparing the molecular sieve coating slurry does not include the step of adjusting pH.
[0024] According to the present invention, the method for preparing the molecular sieve coating slurry does not include an aging step.
[0025] According to the present invention, the slurry obtained after ball milling and dispersion forms a stable and uniform mixed liquid, which is the coating slurry.
[0026] According to the present invention, the ball mill is a planetary ball mill, and the mass of the zirconium balls of the planetary ball mill is 4-6 times the mass of the molecular sieve; further preferably, the mass of the zirconium balls is 5 times the mass of the molecular sieve.
[0027] According to the present invention, the setting parameters of the planetary ball mill are 250-350 rpm, and the dispersion time is 5-60 min; further preferably, the setting parameters of the planetary ball mill are 300 rpm, and the dispersion time is 30 min. Optionally, the carrier of the monolithic catalyst is cordierite honeycomb ceramic.
[0028] The present invention also includes the molecular sieve coating slurry prepared by the above method.
[0029] The present invention also includes the use of the molecular sieve coating slurry in preparing an integral catalyst.
[0030] The present invention also provides a monolithic catalyst, comprising a carrier cordierite honeycomb ceramic, and the molecular sieve coating slurry coated on the carrier. Optionally, the loading rate of the molecular sieve coating slurry on the carrier is 32-37 wt%.
[0031] The present invention also provides a method for preparing the above-mentioned integral catalyst, comprising: providing a carrier cordierite honeycomb ceramic, and coating the above-mentioned molecular sieve coating slurry onto the carrier.
[0032] Different from the prior art method of using aluminum sol, alkaline silica sol, zirconium sol as a binder or dissolving aluminum sol dry powder in water first, the present invention selects acidic silica sol as a binder, and uses two organic dispersants (polyacrylamide and hydroxymethyl cellulose) to improve the slurry state. At the same time, since the molecular sieve and the acidic silica sol are both acidic, the pH of the slurry is 3-4 after being prepared in a certain proportion, which meets the pH requirement for stable dispersion of the slurry and does not need to adjust the pH. The present invention requires mixing the molecular sieve with the two organic dispersants first, then adding a certain amount of deionized water, and then adding a certain amount of acidic silica sol, and performing ball milling dispersion. The slurry after discharge forms a stable and uniform mixed liquid, which is the coating slurry.
[0033] When aluminum sol is used, there is a gelling process after mixing with water, that is, aluminum sol is positively charged Al2O3 ions uniformly dispersed in water, and aluminum sol has strong thixotropy and viscosity-increasing effects. The viscosity of aluminum sol will increase during storage, but if the aluminum sol is stirred or heated to above 50°C, the viscosity of the colloid will decrease. Therefore, when aluminum sol is used as a binder, the viscosity of the slurry is unstable, and the slurry needs to be aged for a certain period of time before it can be used. At the same time, molecular sieves of different morphologies will affect the aging process. The slurry made from different batches of molecular sieves will also cause different slurry viscosities, further increasing the uncontrollability of the entire process.
[0034] The Zeta potential value of the coating slurry obtained by the preparation method of the present invention is significantly increased compared with the traditional liquid sol, which can be increased from 17.65mv to 58mv, that is, there are more uniformly dispersed positive ions in the coating slurry, and the corresponding molecular sieve coating slurry will not have sedimentation phenomenon, which completely solves the problem of instability and easy sedimentation of molecular sieve slurry.
[0035] In addition, due to the nature of silica sol itself, unlike alumina sol, alumina sol has strong thixotropy and thickening effect. The viscosity of alumina sol will increase during storage, but if the alumina sol is stirred or heated to above 50°C, the viscosity of the colloid will decrease. Therefore, in practical applications, it is necessary to face different requirements of honeycomb ceramic carriers and stir to different degrees to control the viscosity and thus the coating effect. This process is difficult to control. When dealing with molecular sieves between different batches, the slurry may show different performances, resulting in unstable final coating effect. However, silica sol itself does not have thixotropy and is a particularly stable viscosity binder. Using silica sol as a binder can also improve the pore blocking problem of honeycomb ceramic carriers of different specifications. Through laboratory verification, the coating prepared by this method has good stability and good coating strength, that is, a low shedding rate. The coating load rate can reach 36.45% at one time, and the shedding rate can be reduced to less than 1%.
[0036] Since the present invention completely solves the problem of coating slurry stability, the coating slurry can be stored for a certain period of time, up to 6 months without sedimentation, and maintain a stable state, which greatly reduces the difficulty of the coating process, makes the coating process easier to operate, and broadens the operating window of the coating process. At the same time, laboratory tests have verified that the use of silica sol can increase the acid sites of the catalyst coating, so the slurry prepared by this method can improve the NOx conversion efficiency. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with the embodiments. Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The experimental reagents used in the following embodiments, unless otherwise specified, are conventional biochemical reagents; the test methods, unless otherwise specified, are conventional methods.
[0038] The acidic silica sol used in the embodiment of the present invention is an acidic silica sol with a mass fraction of 30% and an average particle size of 10-40nm. It can be a common commercially available acidic silica sol or a homemade one. The homemade method is: dilute the commercially available water glass and exchange it with a cation exchange resin to obtain active silica acid; treat the silica acid with an alkali solution to make it alkaline; then heat the alkaline silica acid solution for condensation reaction and concentrate it to obtain an alkaline silica sol; finally, the alkaline silica sol is subjected to cation exchange through a cation resin, and an appropriate amount of acid is added for adjustment to obtain an acidic silica sol at a corresponding acid value.
[0039] The Cu / SSZ-13 or Cu / SSZ-39 molecular sieve has a silicon-aluminum ratio of 12-20, a Cu loading of 2%-4%, a specific surface area of 500-550m2 / g, a pore volume of 0.26-0.27cm3 / g, a pore diameter of 2.0-2.2μm, and a D90 of 5-8μm.
[0040] Example 1
[0041] A method for preparing a stable molecular sieve coating slurry comprises the following steps:
[0042] 96g of deionized water and 120g of acidic silica sol were mixed and added to the planetary mill, and then 120g of Cu-type SSZ-13 (D90 is 8μm) molecular sieve, 0.16g of hydroxymethyl cellulose, and 0.16g of polyacrylamide were added to the planetary mill, and 630g of zirconium balls were added. After stirring evenly, the mixture was dispersed in a planetary mill for 30 minutes at a speed of 300rpm. After discharging, a stable slurry was formed.
[0043] The zeta potential of the slurry was characterized and the results are shown in Table 1.
[0044] The Zeta potential value of the coating slurry obtained by the method of this embodiment is 58.09mV, which means that it has reached a stable state. The higher the Zeta potential value, the more stable the dispersion system is. Generally, for slurry, when the potential value reaches 30mV, it can be considered to have reached a stable state.
[0045] Example 2
[0046] A method for preparing a stable molecular sieve coating slurry comprises the following steps:
[0047] 96g of deionized water and 120g of acidic silica sol were mixed and added to the planetary mill, and then 120g of Cu-type SSZ-13 (D90 is 5μm) molecular sieve, 0.16g of hydroxymethyl cellulose, and 0.16g of polyacrylamide were added to the planetary mill, and 630g of zirconium balls were added. After stirring evenly, the mixture was dispersed in a planetary mill for 30 minutes at a speed of 300rpm. A stable slurry was formed after discharging.
[0048] The zeta potential of the slurry was characterized and the results are shown in Table 1.
[0049] Example 3
[0050] A method for preparing a stable molecular sieve coating slurry comprises the following steps:
[0051] 96g of deionized water and 120g of acidic silica sol were mixed and added to the planetary mill, and then 120g of Cu-type SSZ-39 (D90 is 8μm) molecular sieve, 0.16g of hydroxymethyl cellulose, and 0.16g of polyacrylamide were added to the planetary mill, and 630g of zirconium balls were added. After stirring evenly, the mixture was dispersed in a planetary mill for 30 minutes at a speed of 300rpm. After discharging, a stable slurry was formed.
[0052] The zeta potential of the slurry was characterized and the results are shown in Table 1.
[0053] Example 4
[0054] A method for preparing a stable molecular sieve coating slurry comprises the following steps:
[0055] 96g of deionized water and 120g of acidic silica sol were mixed and added to the planetary mill, and then 120g of Cu-type SSZ-39 (D90 is 5μm) molecular sieve, 0.16g of hydroxymethyl cellulose, and 0.16g of polyacrylamide were added to the planetary mill, and 630g of zirconium balls were added. After stirring evenly, the mixture was dispersed in a planetary mill for 30 minutes at a speed of 300rpm. After discharging, a stable slurry was formed.
[0056] The zeta potential of the slurry was characterized and the results are shown in Table 1.
[0057] Example 5
[0058] The other conditions were the same as those in Example 1, except that the amount of molecular sieve added was 90 g, the amount of acidic silica sol added was 116.6 g, and the amount of water was 128.3 g, so that the molecular sieve: water ratio in the resulting slurry was 1:2.3, and the silica sol solid content: water ratio was 1:6. The results are shown in Table 1.
[0059] Example 6
[0060] Other conditions were the same as in Example 1, except that the amount of molecular sieve added was 150 g, the amount of acidic silica sol added was 166.6 g, and the amount of water was 33.3 g, so that the molecular sieve: water in the obtained slurry was 1:1, and the solid content of silica sol: water was 1:3. The results are shown in Table 1.
[0061] Comparative Example 1
[0062] A method for preparing a molecular sieve coating slurry comprises the following steps:
[0063] 126g Cu-type SSZ-13 (D90 is 8μm) was mixed with 92.8g deionized water, 116g aluminum sol (solid content is 30%) was added, the pH was adjusted to 3.5, and stirred for 6h to form a stable slurry. The slurry was characterized by Zeta point. The results are shown in Table 1.
[0064] Comparative Example 2
[0065] A method for preparing a molecular sieve coating slurry comprises the following steps:
[0066] 126 g Cu-type SSZ-13 (D90 is 5 μm) was mixed with 92.8 g deionized water, 116 g aluminum sol (solid content is 30%) was added, the pH was adjusted to 3.5, and stirred for 6 hours to form a stable slurry. The slurry was characterized by Zeta point. The results are shown in Table 1.
[0067] Comparative Example 3
[0068] A method for preparing a molecular sieve coating slurry comprises the following steps:
[0069] 126g Cu-type SSZ-39 (D90 is 8μm) was mixed with 92.8g deionized water, 116g aluminum sol (solid content is 30%) was added, the pH was adjusted to 3.5, and stirred for 6h to form a stable slurry. The slurry was characterized by Zeta point. The results are shown in Table 1.
[0070] Comparative Example 4
[0071] A method for preparing a molecular sieve coating slurry comprises the following steps:
[0072] 126g Cu-type SSZ-39 (D90 is 8μm) was mixed with 34.8g deionized water, 174g aluminum sol (solid content is 20%) was added, the pH was adjusted to 3.5, and stirred for 6h to form a stable slurry. The slurry was characterized by Zeta point. The results are shown in Table 1.
[0073] Experimental Example Performance Test
[0074] 1. Potential values of the slurries obtained in the examples and comparative examples:
[0075] Potential value detection method: Use Nanotrac wave II nanoparticle size and Zeta potential instrument for testing.
[0076] Table 1 Zeta potential test results of coating slurries obtained in Examples and Comparative Examples
[0077]
[0078] It can be seen from Table 1 that the Zeta potential values of the slurries obtained in the embodiments of the present invention are greater than those in the comparative examples, and the stability of the slurries is significantly improved. In addition, the planetary mill is used for dispersion, and the dispersion efficiency is high. At the same time, compared with the aluminum sol slurry, the viscosity of the silica sol slurry is more stable and does not require aging, which shortens the pulping time as a whole.
[0079] It can be seen from Examples 1-6 and Comparative Examples 1-4 that the slurry using acidic silica sol as a binder has better stability than that using aluminum sol.
[0080] It can be seen from the above that without going through an aging process, the silica sol slurry can directly reach a stable state, while the slurry potential value of the aluminum sol is relatively low. Therefore, the method of the present invention can greatly shorten the process and improve the stability of the slurry.
[0081] 2. Loading rate and shedding rate of the slurry obtained in the examples and comparative examples
[0082] The test methods for load rate and shedding rate are:
[0083] The resulting slurry was applied on The cordierite honeycomb ceramic with a height of 76.2 mm was dried in a drying oven at 120°C for 1 hour, and then placed in a muffle furnace and calcined at 550°C for 2 hours to obtain a monolithic catalyst and weigh it. The weight minus the weight of the cordierite honeycomb ceramic was divided by the weight of the cordierite honeycomb ceramic to obtain the loading rate. The prepared monolithic catalyst was purged with compressed air at a pressure of 0.6 MPa for 2 minutes and weighed. The reduced mass was divided by the mass of the finished catalyst to obtain the shedding rate. The results are shown in Table 2.
[0084] Table 2 Loading rate and shedding rate of samples
[0085] sample Load factor, % Dropout rate, % Example 1 36.45 0.82 Example 2 35.31 0.42 Example 3 32.89 0.87 Example 4 34.63 0.40 Example 5 33.64 0.08 Example 6 32.28 0.13 Comparative Example 1 29.85 2.69 Comparative Example 2 28.64 2.11 Comparative Example 3 27.36 3.10 Comparative Example 4 30.37 2.88
[0086] As can be seen from Table 2, the loading rate of Example 1 of the present invention is close to that of Comparative Example 1, which are 36.45% and 34.85% respectively. After the catalyst coating is ultrasonically treated, the loading rate of Example 1 of the present invention is about 1.87% lower than that of Comparative Example 1 of the traditional preparation method, indicating that the coating strength of the present invention is also improved without affecting the loading amount.
[0087] It can be seen from Examples 1-6 and Comparative Examples 1-4 that, compared with using aluminum sol, using acidic silica sol as a binder can reduce the shedding rate of the slurry and make the slurry more stable.
[0088] The slurry obtained by the method of the present invention will not affect the loading rate due to uneven coating due to poor stability. Since the slurry has good stability and uniform coating without agglomeration, it is more firmly bonded to the cordierite honeycomb ceramic, thereby reducing the shedding rate.
[0089] 3. Catalytic activity test of samples
[0090] The catalytic performance of the integral catalysts obtained in Examples 1-6 and Comparative Examples 1-4 and the catalysts after purging in Example 1 and Comparative Example 1 were tested. The test conditions were: NH3=500ppm, O2=5vol.%, N2 as the balance gas, and the NOx conversion rate obtained under the conditions of an air velocity of 63000h-1. The test results are shown in Table 3.
[0091] Table 3 Catalytic activity test results of samples
[0092]
[0093] As can be seen from Table 3, the NOx conversion rates of Examples 1-6 of the present invention are higher than those of Comparative Examples 1-4. This may be because the slurry stability of Comparative Examples 1-4 is poor, resulting in uneven coating on the cordierite honeycomb ceramics, causing pore blocking, agglomeration and other phenomena, affecting the catalytic efficiency; on the other hand, due to the poor coating stability of the slurry, the slurry will not be firmly coated on the cordierite honeycomb ceramics, which may cause part of the slurry coating to fall off during the catalytic process, which will also affect the catalytic efficiency. Especially at 200-400°C, it has a higher conversion rate and better high-temperature NH3-SCR performance. The conversion rates of Example 1 and Comparative Example 1 after falling off are both reduced, but the reduction is not large. In addition, the preparation process of the present invention is relatively simple, the process is short, and the aging stage required for the aluminum sol slurry is eliminated. Since the molecular sieve coating slurry prepared by the present invention has a stable viscosity, the viscosity will not change even after stirring, which greatly reduces the difficulty of the coating process and makes the coating process easier to operate.
[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A molecular sieve coating slurry, characterized in that: include: Molecular sieve, polyacrylamide, hydroxymethyl cellulose, acidic silica sol and water; wherein, in the molecular sieve coating slurry, the mass ratio of molecular sieve to water is 1:(1-2.3), and the mass ratio of acidic silica sol to water is 1:(3-6); the average particle size of the acidic silica sol is 10-40nm; in the molecular sieve coating slurry, the mass ratio of molecular sieve to polyacrylamide is (700-800):1, and the mass ratio of molecular sieve to hydroxymethyl cellulose is (700-800):1; in the molecular sieve coating slurry, the mass ratio of polyacrylamide to hydroxymethyl cellulose is 1:(0.8-1.2); the molecular sieve is Cu-SSZ-13 or Cu-SSZ-39, wherein the Cu loading is 2%-4%.
2. The molecular sieve coating slurry according to claim 1, characterized in that: In the molecular sieve coating slurry, the mass ratio of molecular sieve to water is 1:1, 1:1.25, 1:1.5, 1:2, or 1:2.3; and / or the mass ratio of acidic silica sol to water is 1:3, 1:4, 1:5 or 1:
6.
3. The molecular sieve coating slurry according to claim 1 or 2, characterized in that: In the molecular sieve coating slurry, the mass ratio of the molecular sieve to polyacrylamide is 750:1, and the mass ratio of the molecular sieve to hydroxymethyl cellulose is 750:
1.
4. The molecular sieve coating slurry according to claim 1, characterized in that: In the molecular sieve coating slurry, the mass ratio of polyacrylamide to hydroxymethyl cellulose is 1:
1.
5. The molecular sieve coating slurry according to claim 1, characterized in that: The pH of the molecular sieve coating slurry is 3-4; and / or, The potential value of the molecular sieve coating slurry is 54-58 mV.
6. The method for preparing the molecular sieve coating slurry according to any one of claims 1 to 5, characterized in that: include: The molecular sieve, polyacrylamide and hydroxymethyl cellulose are first mixed, and then mixed with water and acidic silica sol, and ball-milled and dispersed to prepare a molecular sieve coating slurry.
7. The method for preparing the molecular sieve coating slurry according to claim 6, characterized in that: The ball mill is a planetary ball mill, and the mass of the zirconium balls of the planetary ball mill is 4-6 times the mass of the molecular sieve.
8. The method for preparing the molecular sieve coating slurry according to claim 7, characterized in that: The mass of zirconium ball is 5 times that of molecular sieve.
9. A molecular sieve coating slurry, characterized in that: Prepared by the method according to any one of claims 6 to 8.
10. Use of the molecular sieve coating slurry according to any one of claims 1 to 5 and 9 in preparing a monolithic catalyst.
11. The use according to claim 10, characterized in that: The carrier of the integral catalyst is cordierite honeycomb ceramic.
12. An integral catalyst, characterized in that: include: A carrier cordierite honeycomb ceramic, and the molecular sieve coating slurry according to any one of claims 1 to 5 and 9 coated on the carrier.
13. The integral catalyst according to claim 12, characterized in that: The loading rate of the molecular sieve coating slurry on the carrier is 32-37 wt %.
14. The method for preparing the integral catalyst according to claim 12 or 13, characterized in that: include: A support cordierite honeycomb ceramic is provided, and the molecular sieve coating slurry is coated on the support.