A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material
By heating and using physical intervention to eliminate gaps, the special-shaped molding of CFRTP is achieved, which solves the problems of high cost and low efficiency in traditional technology, simplifies the process and reduces manufacturing costs, and promotes the application and development of CFRTP.
Patent Information
- Application Number
- CN202310247736.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-15
AI Technical Summary
Traditional continuous fiber reinforced thermoplastic composites (CFRTP) processing technology has high initial costs, high processing temperatures, and high tooling and mold costs. It is difficult to mold complex special-shaped parts. Moreover, the secondary molding process consumes a lot of energy, has low efficiency, and has high manufacturing costs. , restricting its further development and application.
By heating the continuous fiber reinforced thermoplastic composite material block to a soft state, contact and/or non-contact physical methods are used to eliminate the gap with the special-shaped molding surface to ensure that the material block is tightly fitted, and then molded. Production of special-shaped continuous fiber-reinforced thermoplastic composites formed in one go.
It simplifies the process, reduces costs, achieves efficient molding of complex special-shaped parts, reduces the number of molds and machines, and improves production efficiency.
Smart Images

Figure CN116198153B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of continuous fiber reinforced thermoplastic composite material processing, in particular to a method for molding a special-shaped continuous fiber reinforced thermoplastic composite material. Background Art
[0002] Compared with continuous fiber reinforced thermoplastic composites (CFRTP) and continuous fiber reinforced thermosetting composites (CFRP / PCM), the initial cost of traditional CFRTP processing technology is often higher, the processing temperature is higher, the cost of tooling is higher, and its limitations are often magnified, and it is believed that CFRTP is not as good as thermosetting composites. The advantages and utilization value of CFRTP have not been fully recognized and developed due to the lack of key molding technology and equipment, which has hindered the further development and application of CFRTP.
[0003] Compression molding is to cut and stack thermoplastic prepreg, put it into a mold and heat it up. After it reaches the molding temperature, the prepreg layer is pressurized by a press and solidified to obtain a simple plate-shaped product. For complex concave and convex shaped parts, it is difficult to achieve compression molding. Therefore, there are molding processes combining compression molding and injection molding on the market, such as ENGEL's Organomelt process, KraussMaffei's FiberForm process, and Bole's OIHM process. This process is complex and the cost of tooling molds and molding equipment is high, which limits the further development and application of CFRTP.
[0004] Since CFRTP composite materials are solid at room temperature, they are not as soft as continuous fiber reinforced thermosetting composite materials CFRP prepreg PCM. They are easy to lay in the mold and simple to make special-shaped parts. In addition, CFRTP fibers have poor ductility, so the commonly used process is secondary molding. Secondary molding refers to molding CFRTP into a base plate layer (plate-like structure) and placing it in an injection molding tool. Short or long fiber reinforced thermoplastics are then injected into the mold to form an additional layer on or around the CFRTP base layer to form a special-shaped part. This process consumes a lot of energy, has many steps, low efficiency, and high losses. It also increases the number of molds and machines, increasing manufacturing costs. Summary of the invention
[0005] The purpose of the present invention is to provide a method for forming a special-shaped continuous fiber reinforced thermoplastic composite material to solve the problems mentioned in the background technology.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material comprises the following steps:
[0008] Step 1: Prepare the continuous fiber reinforced thermoplastic composite material;
[0009] Step 2: cutting, cutting the continuous fiber reinforced thermoplastic composite material to cut out the required material blocks;
[0010] Step 3: Heating: The cut blocks are heated by a heating device to 180°C-250°C, and the blocks become soft;
[0011] Step 4: Transfer: The heated material block is transferred and placed above the lower mold of the mold, and the upper surface of the lower mold is formed with a special-shaped molding surface;
[0012] Step 5: Eliminating the gap: When the material block is in a soft state, use a contact and / or non-contact physical method to eliminate the gap between the material block and the irregular molding surface to ensure that the material block fits tightly with the irregular molding surface;
[0013] Step 6: Compression molding: Compression molding after eliminating the gap.
[0014] In step 5, the gap can be eliminated by manually pressing with heat-insulating gloves or by pressing with a shaping pressing tool to eliminate the gap between the material block and the irregular molding surface.
[0015] In step 5, the gap can be eliminated by using a high-pressure hot air spray gun to press the material block until it fits the special-shaped molding surface.
[0016] In step 5, the gap can be eliminated by using a shaping box assembly, which includes a robot arm, a box body and a shaping cover; the power output end of the robot arm is connected to the box body; the box body has an inner cavity; the bottom of the box body has an opening; one side of the box body is connected to an inflation valve and an exhaust valve; the shaping cover is made of soft material; the shape of the shaping cover matches the irregular molding surface; and the shaping cover is formed at the opening position.
[0017] The shaping cover can be selected from the following materials: metal sheet, heat-resistant rubber or heat-resistant plastic.
[0018] In step 5, the gap is eliminated by using a shaping frame assembly, which includes a mechanical arm and a shaping frame; the power output end of the mechanical arm is connected to the shaping frame; and shaping blocks are respectively provided on the shaping frame at positions corresponding to the positions to be pressed.
[0019] An intelligent monitoring device is installed on the shaping frame.
[0020] In step 5, a movable module assembly is used to eliminate the gap; the movable module assembly includes an axis, an angle driving device and at least two movable pressure blocks; the axis is installed on the upper template of the mold; the movable pressure blocks are rotatably connected to the axis; the bottom surface of the movable pressure block is a pressing surface that matches the corresponding position of the special-shaped forming surface; the angle driving device is installed between the axis and the movable pressure block to drive the movable pressure block to swing; in step 6, the compression molding uses the movable module assembly to continue the compression molding.
[0021] Furthermore, an inwardly recessed mold cavity is provided between adjacent vertical side walls in the irregularly shaped molding surface.
[0022] The beneficial effects of the present invention are:
[0023] The design heats a block of continuous fiber reinforced thermoplastic composite material into a soft state, and then places it on a lower mold. Physical intervention is used to eliminate the gap between the block and the irregular molding surface of the lower mold. After the block and the irregular molding surface are tightly fitted, compression molding is performed. This method only requires one molding to obtain the desired special-shaped continuous fiber reinforced thermoplastic composite material, and the process is simple and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a structural diagram of the product of the present invention;
[0025] Figure 2 It is a structural diagram of the lower mold of the present invention;
[0026] Figure 3 is a schematic diagram of a gap elimination method in Embodiment 1 of the present invention;
[0027] Figure 4 is a schematic diagram of Embodiment 1 of the present invention after the gap is eliminated;
[0028] Figure 5 is a structural diagram of a shaping box assembly in Embodiment 2 of the present invention;
[0029] Figure 6 is a structural diagram of a shaping frame assembly in Embodiment 3 of the present invention;
[0030] Figure 7 is a structural diagram of the active module assembly before shaping in Example 4 of the present invention;
[0031] Figure 8 It is a schematic diagram of the shaping and gap elimination of the movable module assembly in Embodiment 4 of the present invention;
[0032] Fig. 9 It is a front and back structural diagram of the product of the present invention after molding. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with the accompanying drawings:
[0034] like Figure 1-9 As shown, a method for forming a special-shaped continuous fiber reinforced thermoplastic composite material comprises the following steps:
[0035] Step 1: Prepare the continuous fiber reinforced thermoplastic composite material;
[0036] Step 2: cutting, cutting the continuous fiber reinforced thermoplastic composite material to cut out the required material blocks 100;
[0037] Step 3: Heating: The cut block 100 is heated by a heating device to 180-250 degrees, and the block 100 becomes soft; the 40% PP + 60% glass fiber of the continuous fiber reinforced thermoplastic composite material used in this design heats the block 100 to 220°C, and the heating method is infrared heating.
[0038] Step 4: Transferring: The heated material block 100 is transferred and placed on the lower mold 2 of the mold, and the upper surface of the lower mold 2 is formed with a special-shaped molding surface 21;
[0039] Step 5: Eliminate the gap: When the material block 100 is in a soft state, use contact and / or non-contact physical methods to eliminate the gap between the material block 100 and the irregular molding surface 21 to ensure that the material block 100 and the irregular molding surface 21 fit tightly; the contact method is to press manually or with the help of tools, jigs, etc., and the non-contact method is a high-pressure hot air spray gun.
[0040] Step 6: Compression molding: Compression molding after eliminating the gap.
[0041] like Figure 1-2 As shown, in order to clearly illustrate the processing of various special-shaped shapes, the shape of the product 1 processed in this design includes special-shaped structures such as concave-convex surface 11, deep hole 12, inner right angle 13, outer corner 14, etc.; the special-shaped molding surface 21 in the lower mold 2 matches the shape of the product 1, and a mold cavity 211 is added at the position of the outer corner 14. Since wrinkles will be generated in the part where the material block 100 hangs down, the total thickness of the wrinkles will be three times the thickness of the product 1 itself. These wrinkles will cause the product 1 to: dry yarn, exposed yarn, and lack of material. The present invention provides an inwardly recessed mold cavity 211 between adjacent vertical side walls in the special-shaped molding surface 21, and the wrinkles are absorbed by the mold cavity 211.
[0042] like Fig. 9 As shown, during shaping, the wrinkles are concentrated in the mold cavity 211 and molded into the internal reinforcing ribs 101 of the product 1, while in the remaining corners, the wrinkle positions can also be piled up on the outside to form external reinforcing ribs 102.
[0043] Based on the above processing steps, the method of eliminating the gap can be implemented in the following manner:
[0044] Embodiment 1: Figure 3-4 As shown, direct pressing with heat-insulating gloves 01 and pressing with shaping pressing tools 02 are used to eliminate the gap between the material block 100 and the irregular molding surface 21; a high-pressure hot air spray gun 03 can also be used to press the material block 100 to fit the irregular molding surface 21. The three methods are combined, among which the use of the high-pressure hot air spray gun 03 can not only spray the material block 100 to fit the irregular molding surface 21, but also add heat to the material block 100 to prevent the material block 100 from cooling and hardening. The pressing tool includes a strip pressing block 021 and a deep hole pressing block 022. The strip pressing block 021 is used to press the inner right angle part, and the deep hole 12 part can be pressed by a deep hole pressing block 022 that matches the shape of the deep hole 12. Contact pressing can be used first, and then contact pressing can be used to further eliminate the gap.
[0045] Embodiment 2: Figure 5 As shown, a shaping box assembly is used to eliminate the gap, and the shaping box assembly includes a mechanical arm 3, a box body 4 and a shaping cover 5; the power output end of the mechanical arm 3 is connected to the box body 4; the box body 4 has an inner cavity 401; the bottom of the box body 4 has an opening; one side of the box body 4 is connected with an inflation valve 41 and an exhaust valve 42; the shaping cover 5 is a soft material; the shape of the shaping cover 5 matches the special-shaped molding surface 21; the shaping cover 5 is formed at the opening position; wherein the shaping cover 5 can be selected from the following materials: metal sheet, heat-resistant rubber or heat-resistant plastic. In this embodiment, a beryllium copper sheet is used, wherein the inflation valve 41 can be filled with hot air and cold air, and the exhaust valve 42 is used to extract the air in the inner cavity 401, in order to eliminate the gap. Before the gap is formed, the wrinkles on the drooping part are first stuffed into the mold cavity 211 manually or through an external robot arm, and then the robot arm 3 drives the box to move above the material block 100 of the lower mold 2, and then hot air is repeatedly introduced into the inner cavity 401, and the air in the inner cavity 401 is extracted. After the hot air is introduced, the shaping hood 5 is stretched outward to shape the material block 100. After the air is extracted, the shaping hood 5 shrinks inward. Due to the introduction of hot air, the material block 100 can be kept warm during the shaping process, thereby reducing its cooling efficiency. After repeated shaping, the material block 100 is completely fitted with the irregular molding surface 21. After the gap is eliminated, cold air is injected into the inner cavity 401 to cool the material block 100 and solidify the material block 100.
[0046] Example 3: Figure 6As shown, the method for eliminating the gap is to use a shaping frame assembly, and the shaping frame assembly includes a robot arm 3 and a shaping frame 6; the power output end of the robot arm 3 is connected to the shaping frame 6; the shaping frame 6 is provided with shaping blocks 61 at the positions corresponding to the positions to be pressed, and the shaping blocks 61 are set at specific positions according to the shaping position and shape, and then the robot arm is used to control the shaping frame 6 to move up and down and left and right, so that the material block 100 can be shaped to eliminate the gap. Before using the shaping frame assembly for shaping, the wrinkles of the subordinate parts can be stuffed into the mold cavity 211 manually or with the help of an external robot.
[0047] The shaping frame 6 is equipped with an intelligent monitoring device 62, which includes monitoring technologies such as laser radar, temperature detector, and video detection, to monitor and analyze the shaped material block 100, and then take relevant measures according to the analysis results: 1) temperature compensation, the temperature detector detects the temperature, and by setting an infrared heating lamp on the shaping frame 6, the temperature of the material block 100 with uneven temperature or local low temperature / loss of temperature is compensated; 2) video detection is used to find wrinkles, and the wrinkles are inserted into the mold blood by a robot or manually to be flattened; 4) laser radar is used to detect whether the thickness of the material block 100 is sufficient, and material is supplemented / added / stacked at insufficient positions. The shaping frame 6 can be integrated with a material filling port to improve efficiency.
[0048] Example 4: Figure 7-8 As shown, the method of eliminating the gap adopts a movable module assembly; the movable module assembly includes an axis 7, an angle driving device and at least two movable pressing blocks 8; the axis 7 is installed on the upper template of the mold; the movable pressing blocks 8 are all rotatably connected to the axis 7; the bottom surface of the movable pressing block 8 is a pressing surface that matches the corresponding position of the irregular molding surface 21; the angle driving device is installed between the axis 7 and the movable pressing block 8, and is used to drive the movable pressing block 8 to swing. In this embodiment, two movable pressing blocks 8 are disclosed, and the two movable pressing blocks 8 are distributed left and right and open outward at an angle of 30-45°; before eliminating the gap, the wrinkles are placed in the mold cavity 211 manually or by an external manipulator, and then the upper mold drives the axis 7 to move downward, and the angle driving device drives the two movable pressing blocks 8 to swing inward, and the material block 100 is pressed on the irregular molding surface 21 of the lower mold 2, thereby eliminating the gap. In step 6, the compression molding adopts the movable module assembly to continue the compression molding.
[0049] Compared with the conventional mold pressing, the upper mold descends vertically to close the mold with the lower mold, and the vertical movement causes hard contact between the mold wall and the material block 100. The material block 100 on the outer side of the edge is also pressed at the same time, and it is impossible to add material to the inside. The inside and the outside are pressed at the same time, pulling each other and breaking the fiber. In this embodiment, the movable pressing block 8 cuts in at an angle of 30 to 45 degrees, pushing the material sheet to the mold wall, and at the same time, the material sheet on the outer side of the edge has not been pressed yet, and can be added in time without causing "hard pulling" between each other.
[0050] The above description does not limit the technical scope of the present invention in any way. Any modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material, It is characterized in that The following steps are involved: Step 1: Prepare the continuous fiber reinforced thermoplastic composite material; Step 2: cutting, cutting the continuous fiber reinforced thermoplastic composite material to cut out the required material blocks; Step 3: Heating: The cut blocks are heated by a heating device to 180°C-250°C, and the blocks become soft; Step 4: Transfer: The heated material block is transferred and placed above the lower mold of the mold, and the upper surface of the lower mold is formed with a special-shaped molding surface; Step 5: Eliminating the gap: When the material block is in a soft state, a contact and / or non-contact physical method is used to eliminate the gap between the material block and the irregularly shaped molding surface to ensure that the material block and the irregularly shaped molding surface are closely fitted; it also includes a wrinkle finishing process, in which an inwardly concave mold cavity is provided between adjacent vertical side walls in the irregularly shaped molding surface, and the wrinkles generated by the overlapping of the material blocks are stuffed into the mold cavity to form reinforcing ribs on the product; Step 6: Compression molding: Compression molding after eliminating the gap.
2. A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 1, Features: In step 5, the gap is eliminated by manually pressing with heat-insulating gloves and by pressing with a shaping pressing tool to eliminate the gap between the material block and the irregular molding surface.
3. The method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 1, Features: In step 5, the gap is eliminated by using a high-pressure hot air spray gun to press the material block until it fits the irregular molding surface.
4. The method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 1, Features: In step 5, the gap is eliminated by using a shaping box assembly for shaping, the shaping box assembly includes a mechanical arm, a box body and a shaping cover; the power output end of the mechanical arm is connected to the box body; the box body has an inner cavity; the bottom of the box body has an opening; one side of the box body is connected to an inflation valve and an exhaust valve; the shaping cover is made of soft material; the shape of the shaping cover matches the irregular molding surface; The shaping cover is formed at the opening position.
5. A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 4, Features: The shaping cover can be selected from the following materials: metal sheet, heat-resistant rubber or heat-resistant plastic.
6. A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 1, Features: In step 5, the gap is eliminated by using a shaping frame assembly, which includes a mechanical arm and a shaping frame; the power output end of the mechanical arm is connected to the shaping frame; and shaping blocks are respectively provided on the shaping frame at positions corresponding to the positions to be pressed.
7. A method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 6, Features: An intelligent monitoring device is installed on the shaping frame.
8. The method for forming a special-shaped continuous fiber reinforced thermoplastic composite material according to claim 1, Features: In step 5, a movable module assembly is used to eliminate the gap; the movable module assembly includes an axis, an angle driving device and at least two movable pressure blocks; the axis is installed on the upper template of the mold; the movable pressure blocks are rotatably connected to the axis; the bottom surface of the movable pressure block is a pressing surface that matches the corresponding position of the special-shaped forming surface; the angle driving device is installed between the axis and the movable pressure block to drive the movable pressure block to swing; in step 6, the compression molding uses the movable module assembly to continue the compression molding.
Citation Information
Patent Citations
Method for moulding and designing cabin body of composite material
CN108099080A
Preparation method for continuous fiber-reinforced thermoplastic composite seat base plate front end part
CN110614746A
Composite material rib forming mold and forming method
CN112549581A
Preparation of vehicle bottom guard plate based on continuous fiber thermoplastic composite material one-way belt
CN114311468A