A method for preparing macroporous hydrogel by reverse initiation inverse high internal phase Pickering emulsion template method

Through the reverse-initiated high internal phase Pickering emulsion template method, monomer aqueous solution and dumbbell-shaped Janus nanoparticles are used to replace traditional surfactants, which solves the problems of poor biocompatibility and low mechanical strength of macroporous hydrogels in traditional methods. Macroporous hydrogels with high pore size uniformity and high porosity are prepared, which are suitable for applications in the fields of biomedicine and tissue engineering.

CN116199823BActive Publication Date: 2024-10-18ZHEJIANG UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211692256.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-18
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The traditional high internal phase emulsion template method requires a large amount of organic solvents and surfactants when preparing macroporous hydrogels, resulting in poor biocompatibility, uneven pore size distribution, and low mechanical strength, which limits its application in the fields of biomedicine and tissue engineering. application.

Method used

The reverse-initiated reverse-phase high internal phase Pickering emulsion template method is used, using monomer aqueous solution as the internal phase droplet template, the initiator is dissolved in the external oil phase, and dumbbell-shaped Janus nanoparticles are used as surface-active substances to replace traditional surfactants. A high internal phase Pickering emulsion is prepared to form a water-in-oil emulsion, which reduces the use of organic solvents and improves pore size uniformity.

Benefits of technology

It achieves the preparation of macroporous hydrogels with high pore size uniformity and high porosity, reduces the use of organic solvents, and improves mechanical strength. It is suitable for applications in the fields of biomedicine and tissue engineering, and is in line with the development concept of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116199823B_ABST
    Figure CN116199823B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a macroporous hydrogel by a reverse initiation inverse high internal phase Pickering emulsion template method. The specific operation method is to disperse an initiator and dumbbell-shaped amphiphilic Janus nanoparticles in an organic solvent, obtain an oil phase after the initiator is completely dissolved, dissolve a monomer and a cross-linking agent in deionized water to prepare an aqueous solution, obtain an aqueous phase after the monomer and the cross-linking agent are completely dissolved, add the aqueous phase to the oil phase, and then perform high-speed homogenization to obtain a uniform reverse high internal phase Pickering emulsion, deoxygenate after sealing, and then perform polymerization and cross-linking reactions. After the reaction is completed, ethanol is used as an extractant to remove the internal phase by extraction, and the macroporous hydrogel as a whole is obtained after freeze drying. The present invention utilizes the unique advantages of the reverse initiation inverse high internal phase Pickering emulsion template method, uses a small amount of organic solvent, is green and environmentally friendly, and prepares a hydrogel as a whole with high mechanical strength and non-dispersed particles; a macroporous hydrogel with high pore uniformity, large pore size, high porosity, and easily regulated pore structure can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous polymer material preparation, and in particular relates to a method for preparing macroporous hydrogel by a reverse-initiated inverse high internal phase Pickering emulsion template method. Background Art

[0002] Hydrogel is a functional polymer material with a three-dimensional network structure that is composed of a polymer main chain and hydrophilic functional groups, integrating water absorption and water retention. Since Wicherle and Lim proposed the concept of hydrogel in 1960, hydrogel has now developed into an important class of polymer materials. Due to its good adsorption performance and biocompatibility, hydrogel has received extensive attention and attention in the fields of biomaterials and medicine. Common hydrogels include polyacrylamide, polyvinyl alcohol, polyacrylic acid and derivatives. According to the pore size range, hydrogels can be divided into: microporous hydrogels (10-100nm) and macroporous hydrogels (>0.1μm). Macroporous hydrogels have the advantages of high permeability, low mass transfer resistance, low operating pressure, and fast adsorption / desorption rate. They have important applications in protein separation, tissue engineering, drug release, adsorption and sensors. The methods commonly used to prepare macroporous hydrogels are: low-temperature freezing crystallization pore making method, porogen method, phase separation method, foaming method, and emulsion template method. The first four methods are difficult to control the pore size, shape, distribution or orientation of the hydrogel, and the prepared hydrogels have problems such as poor open porosity and unsatisfactory pore structure. The high internal phase emulsion (HIPEs) template method, that is, the droplet template with an emulsion internal phase volume fraction greater than 74%, has the ability to prepare hydrogels with a truly continuous, open macroporous structure, which can form a network with high porosity, which is conducive to transportation and cell scaffold applications. This method has the advantages of simple manufacturing process, easy operation, short time (4-6h), and low energy consumption (50-60°C). However, the implementation of this method requires the use of a large amount of organic solvents and surfactants, which is extremely unfavorable for applications in life science fields such as biocompatibility, biomedicine, cell culture and tissue engineering. Therefore, on this basis, it is necessary to develop a method for preparing an overall macroporous hydrogel using a monomer aqueous solution as a template, only a small amount of organic solvent as a continuous phase, without the participation of traditional surfactants, with controllable morphology and excellent performance.

[0003] Traditionally, the emulsion type used to prepare overall macroporous hydrogels using HIPEs as templates is the oil-in-water (O / W) type, that is, the water phase is the continuous phase and the oil phase is the dispersed phase. Although this method can prepare macroporous hydrogels with open pores, the biggest disadvantage of this method is that it requires the use of a large amount of organic solvents and organic surfactants, which has a heavy environmental burden. Secondly, the hydrogels prepared by this method are mostly hierarchical porous structures composed of primary pores (cavities) and secondary pores, among which the secondary pores are small in size and some of the pores are closed pores, which leads to the defects of a wide overall pore size distribution range, poor pore size uniformity and low porosity of the hydrogel. On the other hand, in HIPEs, the monomer aqueous solution is used as the continuous phase, and its volume fraction is less than 26%. The small amount of monomer aqueous solution leads to lower mechanical strength of the resulting hydrogel, which greatly limits the application of macroporous hydrogels in specific fields such as support materials, adsorption, separation, and catalysis. Summary of the invention

[0004] In order to solve the many problems existing in the traditional preparation of macroporous hydrogels using HIPEs as templates, the purpose of the present invention is to provide a method for preparing macroporous hydrogels by reverse inversion high internal phase Pickering emulsion template method. An aqueous solution of monomers (such as AM, HEMA, HEA, NIPAM, MAA, AA, etc.) is used as an internal phase droplet template, and an initiator (such as AIBN, BPO) is dissolved in the external oil phase. Based on existing laboratory research, a dumbbell-shaped Janus nanoparticle with amphiphilicity is designed and used as a surfactant to replace traditional surfactants to prepare a high internal phase Pickering emulsion, namely, reverse inversion high internal phase Pickering emulsion (ii-HIPPEs). Reverse inversion high internal phase Pickering emulsion is defined as an oil-in-water (i.e., W / O, water phase is dispersed phase, oil phase is continuous phase) type emulsion with a dispersed phase volume fraction (internal phase) greater than or equal to 74%, and a monomer aqueous solution is used as the internal phase of the emulsion, and the initiator is dissolved in the oil phase.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing macroporous hydrogel by reverse initiation inverse high internal phase Pickering emulsion template method, the specific steps are as follows:

[0007] (1) dispersing an initiator and dumbbell-shaped amphiphilic Janus nanoparticles in an organic solvent, and obtaining an oil phase after the initiator is completely dissolved;

[0008] (2) dissolving the monomer and the cross-linking agent in deionized water to prepare an aqueous solution, and obtaining an aqueous phase after the monomer and the cross-linking agent are completely dissolved;

[0009] (3) adding the aqueous phase obtained in step (2) to the oil phase obtained in step (1), and then performing high-speed homogenization to obtain a uniform inverse high internal phase Pickering emulsion;

[0010] (4) The inverse high internal phase emulsion obtained in step (3) is sealed and deoxygenated, and then subjected to polymerization and cross-linking reactions. After the reaction is completed, ethanol is used as an extractant to remove the internal phase by extraction, and the macroporous hydrogel is obtained after freeze-drying.

[0011] Furthermore, the initiator in step 1) is azobisisobutyronitrile, dibenzoyl peroxide, dodecyl peroxide or diisopropylbenzene peroxide.

[0012] Furthermore, in step 1), the mass fraction of dumbbell-shaped amphiphilic Janus nanoparticles in the oil phase is 2.7-7.6%.

[0013] Furthermore, the organic solvent in step 1) is toluene, xylene, n-hexane or n-octane.

[0014] Furthermore, in step 1), the volume fraction of the organic solvent is 15-25% of the total volume of the emulsion.

[0015] Furthermore, in step 2), the monomer is acrylamide, methacrylic acid, acrylic acid, N-isopropylacrylamide, hydroxyethyl methacrylate or hydroxyethyl acrylate.

[0016] Furthermore, in step 2), the cross-linking agent is N,N-methylenebisacrylamide.

[0017] Furthermore, the mass fraction of the monomer in the water phase is 25-40%, and the mass fraction of the cross-linking agent in the water phase is 0.26-0.3%.

[0018] Furthermore, in step 3), the volume fraction of the internal phase in the inverse high internal phase Pickering emulsion is 75-85%. The beneficial effects of the present invention are mainly manifested in:

[0019] (1) The present invention develops a method for preparing macroporous hydrogels by reverse initiation inverse high internal phase Pickering emulsion template method, which provides a new idea for the method of preparing macroporous structure hydrogels by emulsion template method and expands the application scope of reverse emulsion template method. Therefore, it has important significance in the field of macroporous hydrogels.

[0020] (2) The unique advantages of the reverse-initiated inverse high internal phase Pickering emulsion template method are: first, the amount of organic solvent used is small, and no traditional surfactants are used, which is green and environmentally friendly, less polluting, and conducive to sustainable development; second, a hydrogel with high mechanical strength and non-dispersed particles can be prepared as a whole; third, a macroporous hydrogel with high pore uniformity, large pore size, high porosity, and easily controllable pore structure can be obtained, which is conducive to the further application of porous hydrogels.

[0021] (3) This method is simple, time-saving (4-6 h), low energy consumption (reaction at 50 °C), and in line with the concept of green chemistry development.

[0022] (4) The implementation scheme shows that the amount of organic solvent added in the prepolymerized emulsion system prepared by the present invention is reduced by more than 66% compared with the amount of organic solvent used in the traditional emulsion template method.

[0023] (5) The results of scanning electron microscopy tests show that the average pore size of the macroporous hydrogels prepared by the present invention is almost all greater than 4 μm, which is more than twice the pore size of the hydrogels prepared by the traditional method, and the porosity is as high as more than 70%. Compared with the macroporous hydrogels prepared by the traditional method, the porosity is increased by more than 27%.

[0024] (6) The compressive stress-strain curve test shows that the macroporous hydrogel prepared by the present invention and the macroporous hydrogel prepared by the reverse initiation inverse high internal phase surfactant emulsion template method exhibit the same high compressive strength, and both have higher compressive strength than the macroporous hydrogel prepared by the traditional method. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the appearance of the hydrogel sample prepared by the traditional high internal phase emulsion template method;

[0026] Figure 2 This is the appearance of the hydrogel sample prepared by the reverse initiation inverse high internal phase surfactant emulsion template method;

[0027] Figure 3 This is the appearance of the hydrogel sample prepared by the reverse-initiated inverse high internal phase Pickering emulsion template method;

[0028] Figure 4 This is the TEM image of dumbbell-shaped Janus nanoparticles;

[0029] Figure 5 The SEM images of the macroporous hydrogels prepared in Examples 1 to 9, wherein a: Example 1; b: Example 2; c: Example 3; d: Example 4; e: Example 5; f: Example 6; g: Example 7; h: Example 8; i: Example 9;

[0030] Figure 6The SEM images of the macroporous hydrogels prepared in Comparative Examples 1 and 2, wherein a: Comparative Example 1, b: Comparative Example 2;

[0031] Figure 7 Mechanical property test diagrams of PAM hydrogels prepared by the traditional high internal phase emulsion template method (Comparative Example 1), the reverse-initiated inverse high internal phase surfactant emulsion template method (Comparative Example 2) and the reverse-initiated inverse high internal phase Pickering emulsion template method (Example 1). DETAILED DESCRIPTION

[0032] The following examples are only used to further describe the content of the present invention, and are not intended to limit the scope of protection claimed by the present invention. Therefore, any modification or variation based on the present invention should be within the scope of protection claimed by the present invention.

[0033] Example 1

[0034] First, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surface active substances, the TEM image of which is shown in FIG. Figure 4 As shown in the figure, the initiator and Janus nanoparticles were dispersed in 2 ml toluene to obtain an oil phase, and the mass fraction of the initiator and Janus nanoparticles in the oil phase was 4.2%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, the mass fraction of the monomer in the aqueous phase was 30%, and the mass fraction of the crosslinker in the aqueous phase was 0.3%; the aqueous phase was added to the oil phase, and a high-speed homogenizer was used to homogenize at 10000rpm for 1min to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%, and then, it was sealed and deoxygenated with N2 for 15min, and then placed in an oil bath at 50℃ for polymerization, and the crosslinking reaction was performed for 6h to obtain the hydrogel as a whole; ethanol was used as the extractant, toluene was removed by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying. Compared with the porosity of the hydrogel prepared by the conventional method in Comparative Example 1, the porosity is increased by 27%, and the average pore size is increased from 2.87 μm to 9.12 μm, as shown in Table 1. The mechanical strength shows the same high compressive strength as the macroporous hydrogel prepared by the surfactant-stabilized emulsion in Comparative Example 2, and the compressive strength is higher than that of the macroporous hydrogel prepared by the conventional emulsion template method. Figure 7 In addition, from Figure 3 It can be concluded that the PAM hydrogel prepared by the reverse initiation inverse high internal phase Pickering emulsion template method is a whole hydrogel.

[0035] Example 2

[0036] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 1.6 ml toluene to obtain an oil phase, and the mass fraction of the initiator and Janus nanoparticles in the oil phase was 5.1%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6.4 ml of aqueous phase, and the mass fraction of the monomer in the aqueous phase was 30%, and the mass fraction of the crosslinker in the aqueous phase was 0.28%; the aqueous phase was added to the oil phase, and homogenized at 10000rpm for 1min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 80%, and then, the mixture was sealed and deoxygenated with N2 for 15min, and then placed in an oil bath at 50℃ for polymerization, and the crosslinking reaction was performed for 6h to obtain the hydrogel as a whole; ethanol was used as the extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying. With the increase of dispersed phase volume fraction, the porosity increases from 70% to 75%, such as Figure 5 As shown in b and Table 1.

[0037] Example 3

[0038] First, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 1.2 ml toluene to obtain an oil phase, and the mass fraction of the initiator and Janus nanoparticles in the oil phase was 6.7%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6.8 ml of aqueous phase, the mass fraction of the monomer in the aqueous phase was 30%, and the mass fraction of the crosslinker in the aqueous phase was 0.26%; the aqueous phase was added to the oil phase, and a high-speed homogenizer was used to homogenize at 10000rpm for 1min to obtain an oil-in-water type reverse high internal phase emulsion with an internal phase volume fraction of 85%, and then sealed and deoxygenated with N2 for 15min, and then placed in a 50℃ oil bath for polymerization, and the crosslinking reaction was 6h to obtain a hydrogel as a whole; ethanol was used as an extractant, toluene was removed by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze drying. Compared with Example 2, the porosity was increased by about 3%. Therefore, as the volume fraction of the dispersed phase increases, the porosity of the macroporous hydrogel also increases, e.g. Figure 5 As shown in ac and Table 1.

[0039] Example 4

[0040] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 2 ml toluene to obtain an oil phase, and the mass fraction of the initiator and Janus nanoparticles in the oil phase was 4.2%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fraction of the monomer in the aqueous phase was 25%, and the mass fraction of the crosslinker in the aqueous phase was 0.3%; the aqueous phase was added to the oil phase, and homogenized at 10000rpm for 1min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%, and then, the mixture was sealed and deoxygenated with N2 for 15min, and then placed in an oil bath at 50℃ for polymerization, and the crosslinking reaction was performed for 6h to obtain the hydrogel as a whole; ethanol was used as the extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying. Compared with Example 1, the decrease in the monomer concentration in the aqueous solution did not significantly change the porosity and average pore size. Figure 5 As shown in a and d.

[0041] Example 5

[0042] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 2 ml toluene to obtain an oil phase, and the mass fraction of the initiator and Janus nanoparticles in the oil phase was 4.2%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fraction of the monomer in the aqueous phase was 35%, and the mass fraction of the crosslinker in the aqueous phase was 0.3%; the aqueous phase was added to the oil phase, and homogenized at 10000rpm for 1min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%, and then, the mixture was sealed and deoxygenated with N2 for 15min, and then placed in an oil bath at 50℃ for polymerization, and the crosslinking reaction was performed for 6h to obtain a hydrogel as a whole; ethanol was used as an extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying. Compared with Example 4, the porosity does not change significantly with the increase in the monomer concentration in the aqueous solution, but the average pore size decreases from 9.78 μm to 5.37 μm. Figure 5 As shown in de and Table 1.

[0043] Example 6

[0044] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 2 ml toluene to obtain an oil phase, and the mass fraction of the initiator and Janus nanoparticles in the oil phase was 4.2%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fraction of the monomer in the aqueous phase was 40%, and the mass fraction of the crosslinker in the aqueous phase was 0.3%; the aqueous phase was added to the oil phase, and homogenized at 10000rpm for 1min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%, and then, the mixture was sealed and deoxygenated with N2 for 15min, and then placed in an oil bath at 50℃ for polymerization, and the crosslinking reaction was performed for 6h to obtain a hydrogel as a whole; ethanol was used as an extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying. Compared with Examples 1 and 5, as the concentration of the monomer in the aqueous solution increases, the porosity and average pore size of the prepared hydrogel decrease to 66% and 4.83 μm, respectively. Figure 5 As shown in a, e, f and Table 1.

[0045] Example 7

[0046] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 2 ml toluene to obtain an oil phase, and the mass fractions of the initiator and Janus nanoparticles in the oil phase were 4.3% and 2.7%, respectively. Acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fractions of the monomer and the crosslinker in the aqueous phase were 30% and 0.3%, respectively. The aqueous phase was added to the oil phase and homogenized at 10000 rpm for 1 min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%. Then, the mixture was sealed and deoxygenated with N2 for 15 min, and then placed in an oil bath at 50°C for polymerization. The crosslinking reaction lasted for 6 h to obtain a hydrogel as a whole. Ethanol was used as an extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water. After freeze-drying, a macroporous hydrogel with a porous structure was obtained. Compared with Example 1, the reduction in the amount of surfactant added caused a significant change in porosity and pore size, with the porosity decreasing to 59% and the average pore size increasing to 38.53 μm. Figure 5 As shown in g.

[0047] Example 8

[0048] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 2 ml toluene to obtain an oil phase, and the mass fractions of the initiator and Janus nanoparticles in the oil phase were 4.2% and 5.2%, respectively; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fraction of the monomer in the aqueous phase was 30%, and the mass fraction of the crosslinker in the aqueous phase was 0.3%; the aqueous phase was added to the oil phase, and homogenized at 10000rpm for 1min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%, and then, the mixture was sealed and deoxygenated with N2 for 15min, and then placed in an oil bath at 50℃ for polymerization, and the crosslinking reaction was performed for 6h to obtain the hydrogel as a whole; ethanol was used as the extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying. Compared with Example 7, the increase in the amount of surfactant added increased the porosity to 71%, while the average pore size decreased to 7.17 μm. Figure 5 As shown in h.

[0049] Example 9

[0050] Firstly, azobisisobutyronitrile initiator and amphiphilic dumbbell-shaped Janus nanoparticles (surfactant) were dispersed in 2 ml toluene to obtain an oil phase, and the mass fractions of the initiator and Janus nanoparticles in the oil phase were 4.1% and 7.6%, respectively. Acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fractions of the monomer and the crosslinker in the aqueous phase were 30% and 0.3%, respectively. The aqueous phase was added to the oil phase and homogenized at 10000 rpm for 1 min using a high-speed homogenizer to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%. Then, the mixture was sealed and deoxygenated with N2 for 15 min, and then placed in an oil bath at 50°C for polymerization. The crosslinking reaction lasted for 6 h to obtain a hydrogel as a whole. Ethanol was used as an extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water. After freeze-drying, a macroporous hydrogel with a porous structure was obtained. Compared with Examples 1 and 8, as the surfactant increases, the porosity of the macroporous hydrogel increases and the pore size decreases. Figure 5 As shown in a, h, i and Table 1.

[0051] Comparative Example 1

[0052] First, ammonium persulfate initiator, Tween 80 nonionic surfactant (emulsifier), acrylamide monomer, and N,N-methylenebisacrylamide crosslinker are dissolved in deionized water to obtain 2 ml of aqueous phase, the mass fraction of initiator and emulsifier in the aqueous phase is 4.2%, the mass fraction of monomer aqueous solution is 30%, and the mass fraction of crosslinker in the aqueous phase is 0.3%. 6 ml of toluene is taken as the oil phase; the oil phase is added to the aqueous phase, and a high-speed homogenizer is used to homogenize at 10000rpm for 1min to obtain a water-in-oil type high internal phase emulsion with an internal phase volume fraction of 75%. Then, it is sealed and deoxygenated with N2 for 15min, and then placed in a 50℃ oil bath for polymerization. The crosslinking reaction is performed for 6h to obtain a hydrogel as a whole; ethanol is used as an extractant to remove toluene by extraction, and the surface of the hydrogel is rinsed with deionized water. After freeze-drying, a macroporous hydrogel with a porous structure is obtained, such as Figure 6 As shown in a, its appearance is Figure 1 shown.

[0053] Comparative Example 2

[0054] First, azobisisobutyronitrile initiator and Span80 nonionic surfactant (emulsifier) ​​were dissolved in 2 ml toluene to obtain an oil phase, and the mass fraction of the initiator and the emulsifier in the oil phase was 4.2%; acrylamide monomer and N,N-methylenebisacrylamide crosslinker were dissolved in deionized water to obtain 6 ml of aqueous phase, and the mass fraction of the monomer in the aqueous phase was 30%, and the mass fraction of the crosslinker in the aqueous phase was 0.3%; the aqueous phase was added to the oil phase, and a high-speed homogenizer was used to homogenize at 10000rpm for 1min to obtain an oil-in-water type inverse high internal phase emulsion with an internal phase volume fraction of 75%, and then, the mixture was sealed and deoxygenated with N2 for 15min, and then placed in a 50℃ oil bath for polymerization, and the crosslinking reaction was performed for 6h to obtain a hydrogel as a whole; ethanol was used as an extractant to remove toluene by extraction, and the surface of the hydrogel was rinsed with deionized water, and a porous macroporous hydrogel was obtained after freeze-drying, such as Figure 6 In addition, from Figure 2 It can be concluded that the PAM hydrogel prepared by the reverse initiation inverse high internal phase surfactant emulsion template method is a whole hydrogel.

[0055] Table 1 Data of macroporous hydrogels prepared under different conditions

[0056] sample Internal phase content Initiator Type Monomer concentration Type of surfactant Amount of surfactant (mg) Porosity Average pore size (μm) Example 1 75% AIBN 30% Janus 80 70 9.12 Example 2 80% AIBN 30% Janus 80 75 7.56 Example 3 85% AIBN 30% Janus 80 77 4.61 Example 4 75% AIBN 25% Janus 80 69 9.78 Example 5 75% AIBN 35% Janus 80 68 5.37 Example 6 75% AIBN 40% Janus 80 66 4.83 Example 7 75% AIBN 30% Janus 50 59 38.53 Example 8 75% AIBN 30% Janus 100 71 7.17 Example 9 75% AIBN 30% Janus 150 73 3.97 Comparative Example 1 75% APS 30% Tween 80 80 55 2.87 Comparative Example 2 75% AIBN 30% Span 80 80 70 4.57

[0057] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the coverage of the present invention.

Claims

1. A method for preparing macroporous hydrogel by reverse initiation inverse high internal phase Pickering emulsion template method, characterized in that The specific steps are as follows: (1) dispersing an initiator and dumbbell-shaped amphiphilic Janus nanoparticles in an organic solvent, and obtaining an oil phase after the initiator is completely dissolved; (2) dissolving the monomer and the cross-linking agent in deionized water to prepare an aqueous solution, and obtaining an aqueous phase after the monomer and the cross-linking agent are completely dissolved; (3) adding the aqueous phase obtained in step (2) to the oil phase obtained in step (1), and then performing high-speed homogenization to obtain a uniform inverse high internal phase Pickering emulsion; (4) sealing and deoxygenating the inverse high internal phase emulsion obtained in step (3), and then subjecting it to polymerization and cross-linking reactions. After the reaction is completed, ethanol is used as an extractant to remove the internal phase by extraction, and freeze-drying to obtain a macroporous hydrogel as a whole; The initiator in step (1) is azobisisobutyronitrile, dibenzoyl peroxide, dodecyl peroxide or diisopropylbenzene peroxide; The organic solvent in step (1) is toluene, xylene, n-hexane or n-octane; In step (1), the organic solvent accounts for 15-25% of the total volume of the emulsion; In step (2), the monomer is acrylamide, methacrylic acid, acrylic acid, N-isopropylacrylamide, hydroxyethyl methacrylate or hydroxyethyl acrylate; In step (2), the cross-linking agent is N,N-methylenebisacrylamide.

2. The method according to claim 1, characterized in that In step (1), the mass fraction of dumbbell-shaped amphiphilic Janus nanoparticles in the oil phase is 2.7-7.6%.

3. The method according to claim 1, characterized in that The mass fraction of the monomer in the water phase is 25-40%, and the mass fraction of the cross-linking agent in the water phase is 0.26-0.3%.

4. The method according to claim 1, characterized in that In step (3), the volume fraction of the internal phase in the inverse high internal phase Pickering emulsion is 75-85%.

Citation Information

Patent Citations

  • Method for preparing porous polymer composite material of ionic liquid functionalization through hole structure from snowman-shaped Janus particles

    CN106496395A