A superhard cemented carbide material and preparation method thereof
By using a mixture of WC, VC and HfC powders for SPS sintering technology, super hard carbide materials with high hardness and good processing performance were prepared, solving the insufficient hardness and wear resistance of existing carbide materials in high-end applications. The problem.
Patent Information
- Application Number
- CN202211681279.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing cemented carbide materials are insufficient in high-end applications, making it difficult to meet the special needs of high-pressure water cutting equipment and other special needs.
Ultra-hard carbide materials are prepared by SPS sintering technology using a mixture of WC, VC and HfC powders, and the powder ratio and sintering parameters are adjusted to improve the relative density, hardness and fracture toughness of the material.
The prepared super hard carbide material has a hardness of 2750HV to 2900HV, a relative density of no less than 99.9%, and has good processing performance, which can better meet the needs of high-end applications.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of powder metallurgy and relates to a method for preparing an inorganic powder material, and more specifically, to a superhard cemented carbide material and a method for preparing the same. Background Art
[0002] Cemented carbide is widely used as a material for various processing tools due to its high hardness and wear resistance, and is known as the "teeth of industry". It meets the development of modern industry and special difficult-to-process materials and is widely used in military industry, aerospace, mechanical processing, metallurgy, oil drilling, mining tools and other fields.
[0003] my country is a major producer and consumer of cemented carbide, but there is a certain gap in the research of cemented carbide materials in high-end fields such as aerospace and medical machinery. Most of the high-precision cemented carbide processing materials rely on imports. In addition, with the development of materials and the emergence of new materials, more and higher requirements are put forward for cemented carbide. For example, in high-pressure water cutting equipment, water and sand flow out through the nozzle made of cemented carbide material. Due to the high pressure of the water cutting machine, the cemented carbide material used in the nozzle needs to have ultra-high hardness and wear resistance.
[0004] At present, my country can independently develop and produce common water jet nozzles, but the domestic high-end water jet nozzle materials have not yet achieved a technological breakthrough. A company in Zhuzhou, China, reported in patent CN 108059460 A "Hard alloy suitable for water jet sand pipe and its preparation method" that the highest hardness of the hard alloy material obtained by the preparation technology of water jet nozzle materials is 2400HV, which cannot meet the requirements of high-end water jet nozzles for material hardness and wear resistance.
[0005] Therefore, making necessary improvements and innovations based on traditional cemented carbide is of great significance to solving the problem of insufficient performance of cemented carbide materials in special applications and improving the service life of cemented carbide materials. Summary of the invention
[0006] The purpose of the present invention is to make up for the deficiencies of the above-mentioned existing research and to provide a superhard cemented carbide material and a preparation method thereof. The cemented carbide material has the advantages of high relative density, ultra-high hardness and good processing performance.
[0007] According to a first aspect of the present invention, a superhard cemented carbide material is provided, which is prepared by SPS sintering a WC+A+B powder mixture, and based on 100wt.% of the total weight of the powder mixture, the powder mixture comprises: 95.0wt.% to 99.5wt.%, preferably 97.0wt.% to 99.5wt.% of WC powder, 0.5wt.% to 5.0wt.%, preferably 0.5wt.% to 3.0wt.% of A+B powder, A is VC, and B is HfC.
[0008] Preferably, the content of A powder is 0.0 wt.% to 3.0 wt.%, more preferably 0.1 wt.% to 3.0 wt.%.
[0009] Preferably, the content of B powder is 0.0 wt.% to 4.0 wt.%, more preferably 0.1 wt.% to 3.0 wt.%.
[0010] It should be noted that the A+B powder here refers to a mixture of one or two selected from A powder and B powder.
[0011] Preferably, the relative density of the cemented carbide material is not less than 99.9%.
[0012] Preferably, the cemented carbide material contains no other impurity phases except the main phase.
[0013] Preferably, the hardness of the cemented carbide material is 2750HV to 2900HV.
[0014] Preferably, the fracture toughness of the cemented carbide material is 4.0 MPa·m 1 / 2 ~8.0MPa·m 1 / 2 , more preferably 6.0 MPa·m 1 / 2 ~8.0MPa·m 1 / 2 .
[0015] According to a second aspect of the present invention, there is provided a method for preparing the superhard cemented carbide material according to the present invention, which comprises the following steps:
[0016] 1) Mixing powder: putting WC powder and A+B powder into a cemented carbide ball mill for ball milling and mixing, and drying the obtained mixed powder. Based on 100wt.% of the mixed powder, the powder mixture comprises: 95.0wt.% to 99.5wt.% of WC powder, 0.5wt.% to 5.0wt.% of A+B powder, A is VC, and B is HfC;
[0017] 2) Mold filling: The alloy powder obtained in step 1) is placed in a graphite female mold and pre-pressed using a hydraulic press with a pre-pressing pressure of 5 to 20 MPa;
[0018] 3) Sintering: Place the assembled graphite mold in the SPS system, set the axial pressure to 10MPa-50MPa, evacuate to below 10Pa, and sinter with electricity; set the heating rate to 50℃-100℃ / min, and the sintering temperature to 1600℃-2000℃, preferably 1700℃-1900℃; end the sintering after keeping warm for 0-5min, and cool with the furnace;
[0019] 4) Sampling: The samples are taken out by a hydraulic press, and the graphite on the surface of the samples is removed by sand blasting to obtain a superhard cemented carbide material.
[0020] Preferably, the WC powder is a commercial pure phase powder with a purity of not less than 99.9% and a powder particle size of 0.1 to 1.0 μm.
[0021] Preferably, the VC powder is a commercial pure phase powder with a purity of not less than 99.9% and a powder particle size of 0.1 to 1.0 μm.
[0022] Preferably, the HfC powder is a commercial pure phase powder with a purity of not less than 99.9% and a powder particle size of 0.1 to 1.0 μm.
[0023] Preferably, the addition ratio of (VC+HfC) is 0.5 wt.% to 3.0 wt.%.
[0024] Preferably, the mixed powder is placed at the center of the graphite mold.
[0025] Preferably, the graphite female mold is separated from the powder by a graphite bushing or graphite paper, and the graphite pressure head is separated from the powder by a graphite sheet or graphite paper; and a layer of graphite felt for heat preservation is wrapped around the periphery of the assembled graphite mold.
[0026] Further preferably, when the sintering temperature is ≤1400°C, the axial pressure is 10-20MPa; when the sintering temperature is greater than 1400°C and less than or equal to 1500°C, the pressure is increased to 20-50MPa, preferably 30-50MPa; constant pressure sintering is performed at the target pressure until sintering is completed.
[0027] Preferably, in step 3), the heating rate is set to 50-100° C. / min.
[0028] Preferably, the relative density of the superhard cemented carbide block material obtained according to the method of the present invention is not less than 99.9%, and the phase does not contain other impurity phases except the main phase.
[0029] Preferably, the hardness of the superhard cemented carbide material obtained according to the method of the present invention is 2750HV to 2900HV.
[0030] Preferably, the fracture toughness of the superhard cemented carbide material obtained by the method of the present invention is 4.0 MPa·m 1 / 2 ~8.0MPa·m 1 / 2 , more preferably 6.0 MPa·m 1 / 2 ~8.0MPa·m 1 / 2 .
[0031] The present invention has the following beneficial effects:
[0032] The invention provides a method for preparing a superhard cemented carbide block material using commercial WC powder, VC powder and HfC powder as raw materials, and the materials are easy to obtain; the invention provides a method for preparing a superhard cemented carbide material using SPS technology after powder mixing, and the method has a simple process, a short production process, and is environmentally friendly; and the prepared cemented carbide material has the advantages of high relative density, ultra-high hardness, and good processing performance. DETAILED DESCRIPTION
[0033] The present invention is further described below by way of examples, but the embodiments of the present invention are not limited thereto.
[0034] In the following examples, the graphite bushing is first matched with the graphite female mold, and then the lower pressure head is placed in the graphite female mold, and a piece of graphite sheet is placed to fit the pressure head; then the mixed powder according to the proportion is loaded into the graphite female mold; finally, the graphite sheet and the upper pressure head are placed in sequence, and the hydraulic press is used to apply pre-pressure and maintain pressure; after the above work is completed, the mold is wrapped with high-temperature graphite felt. The size of the graphite mold and the pressure head is determined by the size of the sample to be prepared.
[0035] The spark plasma sintering system used in the following embodiments is from SINTER LAND Co., Ltd. of Japan, and the models are LABOX-350 and LABOX-6020. Spark plasma sintering (SPS) includes pulse energization pressure sintering, electric field assisted sintering, pulse current rapid sintering, etc. It should be noted that the sintering of cemented carbide materials using the method of the present invention and equipment of other manufacturers and models is also within the scope of the present invention.
[0036] The density results in the following examples were measured using the Archimedes displacement method;
[0037] The hardness test was obtained using a Vickers hardness tester, and the average value of 5 to 10 tests was taken as the final result; the fracture toughness test followed the international standard ISO 28079-2009 "Hardmetals-Palmqvist toughness test", measuring and calculating the total length of the four cracks at the indentation tip, and calculating the fracture toughness K based on the Vickers hardness value of the sample under the indentation. IC .
[0038] Example 1
[0039] The superhard cemented carbide block material of φ50 mm×30 mm was prepared according to the following steps, wherein WC∶VC∶HfC=99∶0.5∶0.5:
[0040] 1) Mixing powder: Put 1000g of the powder weighed in the above weight ratio into a carbide ball milling jar for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the ball milling time is 24h. The powder after ball milling is dried at high temperature in vacuum at 80℃ for 24h.
[0041] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a manual hydraulic press with a pre-pressing pressure of 15 MPa.
[0042] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1820℃; end sintering after 0min of heat preservation, and cool with the furnace. When the temperature reaches 1400℃, increase the pressure gradient to 40MPa.
[0043] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 1.
[0044] Table 1: Performance test results of cemented carbide materials prepared in Example 1
[0045]
[0046] Example 2
[0047] The superhard cemented carbide block material of φ50m×20mm was prepared according to the following steps, wherein WC∶VC∶HfC=98.75∶0.25∶1.0:
[0048] 1) Mixing powder: 700g of the composite powder weighed in proportion is put into a carbide ball mill for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the ball milling time is 24h. The powder after ball milling is dried at high temperature in vacuum at 80℃ for 24h.
[0049] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a hydraulic press with a pre-pressing pressure of 15 MPa.
[0050] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1850℃; end sintering after 1min of heat preservation, and cool with the furnace. When the temperature reaches 1400℃, increase the pressure gradient to 50MPa.
[0051] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 2.
[0052] Table 2: Performance test results of cemented carbide materials prepared in Example 2
[0053]
[0054] Example 3
[0055] The superhard cemented carbide block material of φ100m×30mm was prepared according to the following steps, wherein WC∶VC∶HfC=99.25∶0.25∶0.5:
[0056] 1) Mixing powder: 3800g of the composite powder weighed in proportion is placed in a carbide ball mill for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 4:1, the ball milling speed is 300r / min, and the ball milling time is 48h. The powder after ball milling is dried at high temperature in vacuum at 80°C for 48h.
[0057] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a hydraulic press with a pre-pressing pressure of 15 MPa.
[0058] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1760℃; end sintering after 3 minutes of heat preservation, and cool with the furnace. When the temperature reaches 1400℃, increase the pressure gradient to 40MPa.
[0059] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 3.
[0060] Table 3: Performance test results of cemented carbide materials prepared in Example 3
[0061]
[0062] Example 4
[0063] The superhard cemented carbide block material of φ50 mm×30 mm was prepared according to the following steps, wherein WC∶VC∶HfC=97.0∶1.0∶2.0:
[0064] 1) Mixing powder: Put 1000g of the powder weighed in the above weight ratio into a carbide ball milling jar for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the ball milling time is 24h. The powder after ball milling is dried at high temperature in vacuum at 80℃ for 24h.
[0065] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a manual hydraulic press with a pre-pressing pressure of 15 MPa.
[0066] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1870℃; end sintering after 0min of heat preservation, and cool with the furnace. When the temperature reaches 1400°, increase the pressure gradient to 40MPa.
[0067] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 4.
[0068] Table 4: Performance test results of cemented carbide materials prepared in Example 4
[0069]
[0070] Example 5
[0071] The superhard cemented carbide block material of φ50 mm×10 mm was prepared according to the following steps, wherein WC∶VC∶HfC=98.75∶0.5∶0.75:
[0072] 1) Mixing powder: Put 400g of the powder weighed in the above weight ratio into a carbide ball milling jar for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the ball milling time is 24h. The powder after ball milling is dried at high temperature in vacuum at 80℃ for 36h.
[0073] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a manual hydraulic press with a pre-pressing pressure of 15 MPa.
[0074] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1900℃; end sintering after 0min of heat preservation, and cool with the furnace. When the temperature reaches 1400℃, increase the pressure gradient to 40MPa.
[0075] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 6.
[0076] Table 5: Performance test results of cemented carbide materials prepared in Example 5
[0077]
[0078] Example 6
[0079] The superhard cemented carbide block material of φ100 mm×20 mm was prepared according to the following steps, wherein WC∶VC∶HfC=99.5∶0.25∶0.25:
[0080] 1) Mixing powder: Put 2600g of the powder weighed in the above weight ratio into a carbide ball milling jar for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 3:1, the ball milling speed is 300r / min, and the ball milling time is 24h. The powder after ball milling is dried at high temperature in vacuum at 80℃ for 24h.
[0081] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a manual hydraulic press with a pre-pressing pressure of 15 MPa.
[0082] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1755℃; end sintering after 0min of heat preservation, and cool with the furnace. When the temperature reaches 1400℃, increase the pressure gradient to 40MPa.
[0083] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 6.
[0084] Table 6: Performance test results of cemented carbide materials prepared in Example 6
[0085]
[0086] Comparative Example 1
[0087] According to the patent "Hard alloy suitable for water jet sand pipe and its preparation method", after die pressing, 1700℃ high pressure (pressure of 80MPa) sintering method is used to prepare Mo-doped 2 C, TaC and Cr 3 C 2 The phase composition and some properties of the WC carbide water jet are shown in Table 7.
[0088] Table 7: Performance parameters of cemented carbide materials of Comparative Example 1
[0089]
[0090] Comparative Example 2
[0091] The superhard cemented carbide block material of φ50 mm×30 mm was prepared according to the following steps, wherein WC∶VC∶HfC=85.0∶5.0∶10.0:
[0092] 1) Mixing powder: Put 1000g of the powder weighed in the above weight ratio into a carbide ball milling jar for ball milling. The abrasive is carbide ball, the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the ball milling time is 24h. The powder after ball milling is dried at high temperature in vacuum at 80℃ for 24h.
[0093] 2) Mold filling: The alloy powder obtained after drying in step 1) is placed in a graphite female mold and pre-pressed using a manual hydraulic press with a pre-pressing pressure of 15 MPa.
[0094] 3) Sintering: Place the assembled graphite mold in the SPS sintering system, set the initial axial pressure to 20MPa, evacuate to below 10Pa, start sintering with power on; sinter at a heating rate of 50-100℃ / min, and the sintering temperature is 1820℃; end sintering after 0min of heat preservation, and cool with the furnace. When the temperature reaches 1400℃, increase the pressure gradient to 40MPa.
[0095] 4) Sampling: Take out the sample using a hydraulic press, and remove the graphite on the surface of the sample by sandblasting to obtain a superhard cemented carbide block material. The specific performance parameters are shown in Table 8.
[0096] Table 8: Performance test results of cemented carbide materials prepared in Comparative Example 2
[0097]
Claims
1. A superhard cemented carbide material, wherein: The cemented carbide material is prepared by SPS sintering a WC+A+B powder mixture, based on 100wt.% of the total weight of the powder mixture, the powder mixture comprises: 95.0wt.%~99.5wt.%WC powder, 0.5wt.%~5.0wt.% A+B powder, A is VC, and B is HfC, The relative density of the cemented carbide material is not less than 99.9%.
2. The superhard cemented carbide material according to claim 1, wherein: The powder mixture contains 97.0 wt. % to 99.5 wt. % of WC powder.
3. The superhard cemented carbide material according to claim 1, wherein: The powder mixture contains 0.5 wt.% to 3.0 wt.% of A+B powder.
4. The superhard cemented carbide material according to any one of claims 1 to 3, wherein The hardness of the cemented carbide material is 2750HV to 2900HV; and / or The fracture toughness of the cemented carbide material is 4.0 MPa·m 1 / 2 ~8.0MPa·m 1 / 2 .
5. The superhard cemented carbide material according to claim 4, wherein: The fracture toughness of the cemented carbide material is 6.0 MPa·m 1 / 2 ~8.0MPa·m 1 / 2 .
6. The method for preparing the superhard cemented carbide material according to any one of claims 1 to 5, comprising the following steps: 1) Mixing powder: putting WC powder and A+B powder into a cemented carbide ball mill for ball milling and mixing, and drying the obtained mixed powder. Based on 100wt.% of the mixed powder, the powder mixture comprises: 95.0wt.% to 99.5wt.% of WC powder, 0.5wt.% to 5.0wt.% of A+B powder, A is VC, and B is HfC; 2) Mold filling: The alloy powder obtained in step 1) is placed in a graphite female mold and pre-pressed using a hydraulic press with a pre-pressing pressure of 5 to 20 MPa; 3) Sintering: Place the assembled graphite mold in the SPS system, set the axial pressure to 10-50MPa, evacuate to below 10Pa, and sinter with electricity; set the heating rate to 50℃-100℃ / min, and the sintering temperature to 1600℃-2000℃; end the sintering after 0-5min of heat preservation, and cool with the furnace; 4) Sampling: The samples are taken out by a hydraulic press, and the graphite on the surface of the samples is removed by sandblasting to obtain a superhard cemented carbide block material.
7. The method for preparing a superhard cemented carbide material according to claim 6, wherein: The sintering temperature in step 3) is 1700°C to 1900°C.
8. The method for preparing a superhard cemented carbide material according to claim 6, wherein: The purity of the WC powder is not less than 99.9%, and the powder particle size is 0.1-1.0 μm; The purity of the VC powder is not less than 99.9%, and the powder particle size is 0.1-1.0 μm; The purity of the HfC powder is not less than 99.9%, and the powder particle size is 0.1-1.0 μm.
9. The method for preparing a superhard cemented carbide material according to claim 6, wherein: The WC+A+B mixed powder is placed at the center of the graphite mold.
10. The method for preparing a superhard cemented carbide material according to claim 6, wherein: The graphite female mold and the powder are separated by a graphite bushing or graphite paper, and the graphite pressing head and the powder are separated by a graphite sheet or graphite paper; a layer of graphite felt for heat preservation is wrapped around the assembled graphite mold.
11. The method for preparing a superhard cemented carbide material according to claim 6, wherein: When the sintering temperature is ≤1400°C, the axial pressure is 10-20MPa; when the sintering temperature is greater than 1400°C and less than or equal to 1600°C, the pressure is uniformly increased to 20-50MPa in a gradient pressurization manner; constant pressure sintering is performed at the target pressure until sintering is completed.
12. The method for preparing a superhard cemented carbide material according to claim 11, wherein: When the sintering temperature is greater than 1400° C. and less than or equal to 1600° C., the pressure is uniformly applied to 30-50 MPa in a gradient pressurization manner.
13. The method for preparing a superhard cemented carbide material according to claim 6, wherein: In step 3), the heating rate is set to 50-100° C. / min.
14. A superhard cemented carbide block material, prepared from the cemented carbide material according to any one of claims 1 to 5.
Citation Information
Patent Citations
Hard alloy suitable for abrasive water jet nozzle and preparation method of hard alloy
CN108059460A
SPS sintering method of a large-size non-bonding-phase pure tungsten carbide hard alloy
CN108165859A
Preparation technology of carboloy metal
CN110106423A