A hydrorefining catalyst and its preparation method
By using mesh aluminum oxide support and potassium hydroxide solution pre-spraying method in the hydrorefining catalyst, the gradient distribution of active components is formed, which solves the problems of catalyst deactivation and bed pressure drop, and achieves efficient addition Hydrogen purification treatment and long-life catalyst use.
Patent Information
- Application Number
- CN202111487638.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-06
AI Technical Summary
The existing hydrogenation purification catalyst is prone to inactivation during long-term use, and the bed pressure drops quickly, resulting in frequent shutdown of the hydrogenation device, and it is difficult to achieve high dispersion impregnation of multi-component active components under no heating conditions, which increases preparation cost.
The method of pre-spraying of mesh aluminum oxide support and potassium hydroxide solution is used to form gradient-distributed active components to avoid adsorption heat release, improve the dispersion of active components and the physical and chemical properties of the catalyst, and use alkaline impregnation. The liquid dissolves the active components to ensure efficient dispersion and stability of the catalyst.
It extends the service life of the main catalyst, reduces the coking rate at the top of the bed, improves the impurity filtration capacity, slows down the pressure drop of the bed, and improves the efficiency and product quality of hydrorefining treatment.
Smart Images

Figure CN116212887B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hydrorefining catalyst and a preparation method thereof, and in particular to a hydrorefining catalyst with a protective agent function and a preparation method thereof. Background Art
[0002] Hydrofining technology is the main means to improve the quality of petrochemical products. Hydrofining catalysts and corresponding protective agents are mainly used in the industry today, which are supported catalysts containing active components such as Mo, W, Ni, and Co. The appropriate degree of interaction between the active component and the carrier is one of the main factors affecting the effective loading of the catalyst. Generally speaking, the higher the dispersion of the active component on the carrier, the more effective active sites there are, and the higher the activity of the catalyst. However, the long-term stability of the catalyst must also be considered comprehensively. Therefore, how to improve the interaction between the active component and the carrier to increase the effective loading and dispersion state of the active component on the carrier is the focus of the research and development of hydrofining catalysts.
[0003] Among them, the prepared active component impregnation solution is directly related to the dispersion of the active components in the catalyst after impregnation, thus affecting the performance of the catalyst. The selection of effective solvents and dissolution methods is the key to preparing the impregnation solution. In the process of preparing protective agents containing active components such as molybdenum and cobalt by a one-step impregnation method, the problem with the prior art is that the relative water absorption rate of the protective agent is low. In the process of preparing catalysts by an equal volume impregnation method, the amount of the prepared active component solution is subject to certain restrictions. In the process of preparing catalysts containing components such as molybdenum and cobalt, the main problem is that active components Co, Mo, etc. are difficult to dissolve, especially when dissolving two or more active components in one solvent at the same time. The use of a step-by-step impregnation method will increase the cost of catalyst preparation.
[0004] At present, it is a well-known technology to use ammonia or organic acid as solvent to dissolve active components such as Co, Mo, W, Ni, etc., but ammonia is not effective in improving the dispersion of active components; in comparison, the addition of organic acid will increase the acidity of the catalyst surface, causing the potential risk of coking. In the research on preparation methods and processes, how to simply prepare an impregnation solution containing active components, and achieve the requirements of multi-component one-step impregnation without heating, and keep the active components highly dispersed after impregnation, is still a difficult problem.
[0005] In addition, there are many technical reasons for the shutdown of the hydrotreating unit, but the main reasons are the deactivation of the catalyst and excessive bed pressure drop. Since the particulate matter in the crude oil includes colloids, coke precursors and some harmful substances such as silicon, the sediments formed by the deposition of these substances between the catalyst particles will cause the bed pressure drop to increase, and it often occurs on the catalyst at the top of the reactor that first contacts the raw material. Especially when there is a small amount of iron in the crude oil, once it encounters hydrogen in the presence of sulfur, it will immediately generate gelled iron sulfide. These gelled iron sulfides adhere to or stick to the surface area of the catalyst and between the catalyst particles. At the same time, the iron sulfide will promote the occurrence of coking reaction, aggravating the deactivation of the catalyst and the rate of increase of the bed pressure drop. The above factors often lead to the shutdown of the unit, and the catalyst on the top of the reactor needs to be replaced frequently for "skimming" treatment.
[0006] CN111821965A discloses a carrier, catalyst and preparation method thereof for a hydrogenation protective agent. The carrier is an alumina carrier, including a main alumina and a rod-shaped alumina, wherein the main alumina is an alumina with micron-sized pores, wherein at least part of the rod-shaped alumina is distributed on the outer surface and in the micron-sized pores of the main alumina, wherein the outer surface rod-shaped alumina contains alkali metals and / or alkaline earth metals. The preparation method of the carrier is to first prepare a carrier intermediate, then immerse the carrier intermediate in an ammonium bicarbonate solution, seal and heat treat, dry the material after heat treatment, and then spray and impregnate the material with a solution containing alkali metals and / or alkaline earth metals, and obtain an alumina carrier after drying and roasting. The carrier, as a residual oil hydrogenation protective catalyst, has the characteristics of strong impurity tolerance and high demetallization activity, and is particularly suitable for residual oil hydrogenation treatment processes.
[0007] CN111821990A discloses a residual oil hydrogenation protective agent carrier, catalyst and preparation method thereof. The carrier is a modified alumina-based carrier, and the modified alumina-based carrier contains a modifying element and a first hydrogenation active metal component; the modified alumina-based carrier includes a main modified alumina and a rod-shaped modified alumina, and the main modified alumina is an alumina with micron-sized pores, wherein at least part of the rod-shaped modified alumina is distributed on the outer surface of the main modified alumina and in the micron-sized pores with a pore diameter D of 5 to 10 μm; the modifying element is vanadium, and the first hydrogenation active metal component is molybdenum. It has the characteristics of good macromolecular diffusion performance, strong impurity tolerance, and high asphaltene conversion rate.
[0008] CN102876365B relates to a grading method for a low-quality distillate oil hydrofining catalyst, wherein the reactor is divided into three reaction zones from top to bottom, and a hydrofining protective agent, a hydrofining agent A, and a hydrofining agent B are sequentially loaded; the hydrofining protective agent; uses alumina as a carrier, loads metal Ni and W, and based on the mass of the catalyst, the content of WO3 is 3-10wt%, and the content of NiO is 1-6wt%; the hydrofining agent A; the catalyst is Al2O3-TiO2-SiO2-ZrO2 The catalyst is a ternary composite oxide as a carrier, W-Mo-Ni ternary metal as an active metal component, and P as an additive; Hydrogenation refining agent B; the catalyst is a ternary composite oxide of Al2O3-SiO2-ZrO2 as a carrier, W-Mo-Ni ternary metal as an active metal component, and P and F as additives; based on the overall catalyst mass, the loading amount of the hydrogenation protective agent is 10-30wt%, the loading amount of the hydrogenation refining agent A is 30-60wt%, and the loading amount of the hydrogenation refining agent B is 20-50wt%. The catalysts of different systems are reasonably graded, firstly, the large pore volume, large specific surface area, high surface acid content and highly active ternary metal components of the hydrogenation refining agent A are used to achieve a certain sulfur and deep denitrification effect, and the influence of nitrogen heterocyclic compounds on the desulfurization activity of the subsequent catalyst is weakened, and then through the hydrogenation refining agent B, through the deep desulfurization performance of the catalyst, the ultra-low sulfur diesel with a sulfur content that meets the Euro IV standard is finally obtained.
[0009] CN107875979A discloses a graded filling method and application of a fixed bed hydrogenation catalyst. The graded filling method comprises at least three fixed bed reactors connected in series, and at least one hydrogenation protective agent and at least one first hydrogenation demetallization agent are sequentially filled in the first fixed bed reactor along the logistics direction, wherein a small particle hydrogenation catalyst is filled at the end of the logistics direction. The inventive method can process residual oil raw materials with high iron and calcium content, but is mainly suitable for residual oil hydrogenation units.
[0010] CN1101452C relates to a hydrogenation active protective agent and its preparation method. The carrier used in the protective agent contains both γ-alumina and δ-alumina. The protective agent contains 3-22 wt% of group VIB metal oxide and 0.5-5 wt% of group VIII metal oxide, 0-2 wt% of group IA metal oxide, 0-3 wt% of phosphorus, and a specific surface area of 100-250 m 2 / g, pore volume 0.4~0.8ml / g. It is particularly suitable as a protective agent for inferior heavy crude oil with high sulfur, high nitrogen and high metal content.
[0011] CN1966616B provides a hydrogenation active protective agent and a preparation method thereof, wherein the protective agent comprises an alumina carrier, an effective amount of hydrogenation active metal components and halogens loaded on the carrier, the content of the halogens being 0.5 to 10% by weight based on the element and the catalyst, and the specific surface area of the carrier being 2 to 50 m 2 / g, pore volume 0.4-1.2 ml / g, the carrier is prepared by a method comprising mixing, molding and calcining one or more alumina and / or alumina precursors with at least one halogen-containing compound. However, the hydrogenation protective agent has a small specific surface area and a low content of active components that can be effectively loaded.
[0012] CN101134166B discloses a composite protective agent for hydrogenation catalysts, which is a ceramic composite protective agent body surface with a layer of metal oxide materials containing molybdenum and nickel, the supporting layer is attached to the surface of the composite protective agent body by a granulation method, and then the two are tightly combined to form a composite body through high-temperature sintering. The composite protective agent is porous, which can support the main catalyst in the hydrogenation reaction process and filter the organic impurities in the raw oil to prevent the main catalyst from being poisoned and the pressure drop of the reactor from increasing. At the same time, the supporting layer containing molybdenum and nickel metal oxides of the composite protective agent can also participate in the hydrogenation polymerization reaction to improve the catalytic efficiency. The composite protective agent can be used as a protective agent for catalysts in the crude oil refining hydrogenation reaction of petrochemical industry. Many existing protective agents are ceramic catalyst protective agents, which only play a supporting role and filter larger dirt on the catalyst, and cannot eliminate the effects of colloid and coke precursors in the raw oil and a small amount of metal organic compounds on catalyst poisoning and carbon deposition. In some cases, during the preparation of the protective agent, the compound containing the active metal component is introduced in the form of kneading, so that the molded carrier contains a certain amount of the compound containing the active metal component, so as to simplify the preparation process. However, the method of directly mixing the active metal compound with aluminum hydroxide dry rubber powder or aluminum oxide powder in the form of kneading has problems such as uneven mixing of crystal particles and deterioration of catalyst strength. At the same time, it is not easy for the components to combine to form a specific skeleton structure simply by kneading.
[0013] Therefore, there is an urgent need to develop a hydrotreating catalyst with a protective agent function suitable for being installed on the upper layer of the catalyst to slow down the deactivation rate of the catalyst and the increase rate of the bed pressure drop. Summary of the invention
[0014] The purpose of the present invention is to provide a hydrorefining catalyst and a preparation method thereof. The hydrorefining catalyst has a reasonable distribution of active components, has the function of a hydrogenation protector, can accommodate more particulate matter, and has a certain hydrorefining capacity, can effectively protect the hydrogenation main catalyst, and prolong the service life of the main catalyst.
[0015] To this end, the present invention provides a hydrorefining catalyst, which has the function of a protective agent. The catalyst comprises a carrier, an active component and an auxiliary agent, wherein the active component comprises molybdenum and nickel, the carrier comprises mesh-shaped alumina, and the auxiliary agent is potassium, a part of the potassium is introduced in the form of a carrier pre-spraying, and a part of the potassium is introduced in the form of an active component impregnation liquid, and the carrier after pre-spraying needs to be aged before being impregnated with the active component impregnation liquid;
[0016] Preferably, based on the total weight of the catalyst being 100%, the content of the active component is 5% to 15% and the content of the auxiliary agent is 0.01% to 3%, more preferably 0.1% to 1.5%, calculated on the weight of the corresponding oxide.
[0017] Specifically, the protective agent of the present invention uses a mesh-shaped alumina carrier, which can reduce bed resistance, optimize gas-liquid distribution, efficiently filter impurities and contain colloids, effectively protect the hydrogenation main catalyst, and extend the service life of the main catalyst. At the same time, it can slow down the coking rate on the top of the bed and extend the regeneration cycle. At the same time, it also plays a role in preferentially hydrorefining olefins and impurities such as sulfur and nitrogen in the raw materials.
[0018] Specifically, in the hydrorefining catalyst provided by the present invention, a portion of potassium is added in the form of pre-spraying on the carrier. This portion of potassium plays a role in carrier modification while the carrier is spraying and releasing heat, so that the distribution of the active components of the catalyst has a gradient. This can avoid the process of concentrated release of adsorption heat in the active component impregnation step in the prior art, thereby affecting the dispersion state of the active components in the later stage and the physicochemical properties of the catalyst. In addition, this portion of potassium can also interact with the carrier to reduce the surface acidity of the carrier.
[0019] Specifically, the method of the present invention does not limit the specific composition of the protective agent, and the composition of the active component can be adjusted as needed. Due to the use of the method of the present invention, the protective agent prepared exhibits a more excellent hydrofining effect.
[0020] The hydrorefining catalyst of the present invention is preferably that the mesh-shaped alumina is cylindrical, with a diameter of 10 to 20 mm and a height of 5 to 15 mm; further preferably, the mesh-shaped alumina is honeycomb-shaped, and the specific surface area of the mesh-shaped alumina is 80 to 200 m 2 / g.
[0021] The hydrotreating catalyst of the present invention preferably has an alumina content of ≥80% in the carrier, and the alumina crystal forms include at least two of θ-Al2O3, γ-Al2O3, α-Al2O3, and δ-Al2O3. Specifically, the alumina crystal forms are mainly θ-Al2O3, γ-Al2O3, and may contain α-Al2O3 and δ-Al2O3.
[0022] In the hydrotreating catalyst of the present invention, preferably, the water absorption rate of the carrier is 35wt% to 65wt%, more preferably 50wt% to 60wt%.
[0023] The hydrotreating catalyst of the present invention is preferably pre-sprayed using a spray device, and the pre-spraying is completed within a time range of 1 min to 20 min, more preferably 3 min to 10 min.
[0024] The hydrorefining catalyst of the present invention is preferably used in the carrier pre-spraying process with potassium hydroxide solution, the concentration of the potassium hydroxide solution is 0.1wt% to 5wt%, more preferably 0.5wt% to 1wt%; the amount of the potassium hydroxide solution is: 1%X×T ml to 20%X×T ml, preferably 5%X×T ml to 10%X×T ml, wherein X represents the water absorption rate, and T represents the grams of the pre-sprayed carrier. Specifically, based on the volume of the total impregnation solution (including the potassium hydroxide solution and the active component impregnation solution), the amount of the potassium hydroxide solution, i.e., the volume percentage of the potassium hydroxide solution added, is 1% to 20%, more preferably 5% to 10%.
[0025] Specifically, the potassium hydroxide solution can be prepared by dissolving potassium hydroxide in deionized water in a conventional manner.
[0026] The hydrotreating catalyst of the present invention is preferably prepared by any one of the following methods:
[0027] (1) mixing ammonia water, potassium hydroxide and deionized water to prepare a composite solvent, and adding a salt containing an active ingredient into the composite solvent;
[0028] (2) Ammonia water and deionized water are mixed to prepare a composite solvent, a salt containing an active component is added to the composite solvent, and then potassium hydroxide is added.
[0029] Specifically, the present invention does not impose any particular restrictions on the concentration and amount of ammonia water used to prepare the active component impregnation solution, and conventional selections in the art can be adopted. According to the amount of active component added, each active component can be completely dissolved. The impregnation solution used in the present invention is an alkaline impregnation solution. After the active component is dissolved, the pH value of the impregnation solution needs to be adjusted. The prepared impregnation solution is clear, stable, and has low surface tension and viscosity.
[0030] The hydrotreating catalyst of the present invention is preferably such that, in method (2), the concentration of the potassium hydroxide solution is 0.1wt% to 5wt%, more preferably 0.5wt% to 1wt%; and the amount of the potassium hydroxide solution added is 1% to 20% of the volume of the active component impregnation solution, more preferably 5% to 10%.
[0031] The hydrotreating catalyst of the present invention is preferably prepared in a volume of the active component impregnation solution of 1.05×(1-percentage of potassium hydroxide solution added)X×T ml to 1.25×(1-percentage of potassium hydroxide solution added)X×T ml, and further preferably in a volume of 1.10×(1-percentage of potassium hydroxide solution added)X×T ml to 1.20×(1-percentage of potassium hydroxide solution added)X×Tml, wherein X represents the water absorption rate and T represents the grams of the pre-sprayed carrier.
[0032] The hydrotreating catalyst of the present invention is preferably impregnated at a temperature of 10°C to 30°C, preferably 15°C to 25°C, without the need for a heating process.
[0033] Specifically, the active components are loaded onto the carrier by one-step impregnation, the active components are highly dispersed on the catalyst, and the B acid center on the catalyst is effectively eliminated, and the strong L acid center is weakened. After the active components are loaded, aging, drying and roasting are required. Before impregnating the active components, a certain concentration of potassium hydroxide solution is used to spray the catalyst carrier to release heat and play a role in carrier modification.
[0034] The hydrotreating catalyst of the present invention is preferably added to the active component impregnation solution in the form of ammonium molybdate, and the active component nickel is added to the active component impregnation solution in the form of sulfate, halide, nitrate or acetate, and nitrate and / or acetate are further preferred.
[0035] To this end, the present invention also provides a method for preparing a hydrotreating catalyst, comprising the following steps:
[0036] (1) Pre-spraying and aging the carrier with potassium hydroxide solution;
[0037] (2) preparing an active component impregnation solution containing potassium;
[0038] (3) The aged carrier is immersed in an active component impregnation solution, and then aged, dried, and calcined.
[0039] Specifically, aging, drying and activation are all completed using existing technologies, and the present invention has no special requirements. The conditions and methods of aging, drying and roasting can refer to the existing technology. Preferably, the drying conditions are: temperature 80-120°C, time 2-6 hours, and the roasting conditions are: temperature 350-600°C, time 3-8 hours.
[0040] The beneficial effects of the present invention are as follows:
[0041] The present invention provides a hydrorefining catalyst, which uses a mesh-shaped alumina carrier with high porosity, can efficiently filter impurities, improve the ability to accommodate colloids, and slow down the coking rate on the top of the bed layer, thereby extending the regeneration cycle. At the same time, in the process of loading the active component of the protective agent, the impregnation effect and the active component clustering effect brought by the conventional impregnation method are overcome, the loading effect of the active metal component is improved, the active component forms a certain gradient, and the dispersibility of the active metal on the carrier surface is improved.
[0042] In addition, the present invention finds that the mesh-shaped alumina carrier of the supported catalyst will release a large amount of adsorption heat in a concentrated manner during the impregnation process of the active component impregnation solution, which affects the dispersion state of the active component in the later stage and the physicochemical properties of the catalyst. By pre-spraying potassium hydroxide solution and then impregnating the active component impregnation solution, the hydrogenation performance of the protective agent can be improved. The possible mechanism is: on the one hand, the pre-sprayed potassium hydroxide solution releases part of the adsorption heat of the carrier in advance, so that part of the adsorption heat of the protective agent carrier in the process of impregnating the active component is released in advance; on the other hand, the pre-sprayed potassium hydroxide solution changes the number and arrangement of hydroxyl groups on the surface of the catalyst carrier, which improves the dispersibility of the active component in the subsequent impregnation process of the active component. At the same time, the pre-sprayed solution occupies relatively deep holes in advance due to the capillary effect, so that the active component of the protective agent forms a gradient distribution, and the surface active component is dispersed more efficiently and more evenly. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic diagram of the structure of a mesh-shaped carrier.
[0044] Figure 2 This is the HRTEM component distribution diagram of potassium in the catalyst in Example 2. DETAILED DESCRIPTION
[0045] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments that do not specify specific conditions are usually based on conventional conditions. In the following embodiments, % is mass percentage.
[0046] Example 1
[0047] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 15 mm, a height of 10 mm, and a specific surface area of 117 m 2 / g, water absorption rate is 59%, and the crystal forms are α-Al2O3 and θ-Al2O3.
[0048] Preparation steps of hydrotreating catalyst:
[0049] (1) First, prepare 68 ml of a 0.15 wt% potassium hydroxide solution;
[0050] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for pre-spraying for 3.5 minutes. After the pre-spraying, age it for 12 minutes;
[0051] (3) ammonium molybdate, nickel nitrate, and potassium hydroxide were sequentially added to a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 5) to prepare 628 ml of an active component impregnation solution;
[0052] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 4.5 hours, dried at 100° C. for 4 hours, and calcined at 480° C. for 4 hours to obtain catalyst C1.
[0053] Example 2
[0054] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 12 mm, a height of 10 mm, and a specific surface area of 95 m 2 / g, water absorption rate is 55%, and the crystal form is α-Al2O3 and δ-Al2O3.
[0055] Preparation steps of hydrotreating catalyst:
[0056] (1) First, prepare 50 ml of a 0.5 wt% potassium hydroxide solution;
[0057] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for 2.5 minutes. After spraying, age it for 10 minutes;
[0058] (3) adding ammonium molybdate, nickel chloride and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 6) to prepare 588 ml of an active component impregnation solution;
[0059] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 4 hours, dried at 110° C. for 3 hours, and calcined at 450° C. for 4 hours to obtain catalyst C2.
[0060] Example 3
[0061] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 12 mm, a height of 8 mm, and a specific surface area of 91 m 2 / g, water absorption rate is 54%, and the crystal forms are α-Al2O3 and θ-Al2O3.
[0062] Preparation steps of hydrotreating catalyst:
[0063] (1) First, prepare 32 ml of a 0.6 wt% potassium hydroxide solution;
[0064] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for 3.0 min. After spraying, age it for 8 min;
[0065] (3) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 4) to prepare 594 ml of an active component impregnation solution;
[0066] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 3 hours, dried at 90° C. for 6 hours, and calcined at 500° C. for 4 hours to obtain catalyst C3.
[0067] Example 4
[0068] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 10 mm, a height of 5 mm, and a specific surface area of 158 m 2 / g, water absorption rate is 64%, and the crystal forms are γ-Al2O3 and θ-Al2O3.
[0069] Preparation steps of hydrotreating catalyst:
[0070] (1) First, prepare 86 ml of a 0.3 wt% potassium hydroxide solution;
[0071] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for 8.0 minutes. After spraying, age it for 15 minutes;
[0072] (3) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 3) to prepare 631 ml of active component impregnation solution;
[0073] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 5 hours, dried at 100° C. for 4 hours, and calcined at 400° C. for 5 hours to obtain catalyst C4.
[0074] Example 5
[0075] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 12 mm, a height of 6 mm, and a specific surface area of 98 m 2 / g, water absorption rate is 56%, and the crystal form is γ-Al2O3 and δ-Al2O3.
[0076] Preparation steps of hydrotreating catalyst:
[0077] (1) First, prepare 96 ml of a 0.2 wt% potassium hydroxide solution;
[0078] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for 10 minutes. After spraying, age it for 21 minutes;
[0079] (3) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 6) to prepare 543 ml of active component impregnation solution;
[0080] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 6 hours, dried at 100° C. for 4 hours, and calcined at 520° C. for 5 hours to obtain catalyst C5.
[0081] Example 6
[0082] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 15 mm, a height of 8 mm, and a specific surface area of 85 m 2 / g, water absorption rate is 50%, and the crystal forms are γ-Al2O3, δ-Al2O3, and θ-Al2O3.
[0083] Preparation steps of hydrotreating catalyst:
[0084] (1) First, prepare 18 ml of a 1 wt% potassium hydroxide solution;
[0085] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for 4.5 minutes. After spraying, age it for 5 minutes;
[0086] (3) adding ammonium molybdate, cobalt acetate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 5) to prepare 567 ml of active component impregnation solution;
[0087] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 3 hours, dried at 100° C. for 5 hours, and calcined at 470° C. for 5 hours to obtain catalyst C6.
[0088] Example 7
[0089] The carrier used in this example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 15 mm, a height of 10 mm, and a specific surface area of 82 m 2 / g, water absorption rate is 48%, and the crystal forms are γ-Al2O3, δ-Al2O3, and θ-Al2O3.
[0090] Preparation steps of hydrotreating catalyst:
[0091] (1) First, prepare 41 ml of a 0.4 wt% potassium hydroxide solution;
[0092] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for 6.5 minutes. After spraying, age it for 6 minutes;
[0093] (3) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 4) to prepare 545 ml of an active component impregnation solution;
[0094] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 5 hours, dried at 110° C. for 4 hours, and calcined at 500° C. for 4 hours to obtain catalyst C7.
[0095] Comparative Example 1
[0096] The carrier used in this comparative example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 15 mm, a height of 10 mm, and a specific surface area of 117 m 2 / g, water absorption rate is 59%, and the crystal forms are α-Al2O3 and θ-Al2O3.
[0097] Preparation steps of hydrotreating catalyst:
[0098] (1) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 5) to prepare 696 ml of an active component impregnation solution;
[0099] (2) 1 kg of the mesh-shaped carrier was impregnated into the active component impregnation solution of step (1), aged for 4.5 h, dried at 100° C. for 4 h, and calcined at 480° C. for 4 h to obtain catalyst D1.
[0100] The difference from Example 1 is that the potassium additive is all introduced in the form of active component impregnation solution.
[0101] Comparative Example 2
[0102] The carrier used in this comparative example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 12 mm, a height of 8 mm, and a specific surface area of 91 m 2 / g, water absorption rate is 54%, and the crystal forms are α-Al2O3 and θ-Al2O3.
[0103] Preparation steps of hydrotreating catalyst:
[0104] (1) First, dissolve 15.06 g of potassium hydroxide in distilled water to prepare 50 ml of potassium hydroxide solution;
[0105] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to perform atomization pre-spraying treatment on the carrier for 3.0 minutes. After the pre-spraying, age it for 8 minutes;
[0106] (3) adding ammonium molybdate and nickel nitrate into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 4) to prepare 594 ml of active component impregnation solution;
[0107] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 3 hours, dried at 90° C. for 6 hours, and calcined at 500° C. for 4 hours to obtain catalyst D3.
[0108] The difference from Example 3 is that the potassium additive is all introduced in the form of carrier pre-spraying.
[0109] Comparative Example 3
[0110] The carrier used in this comparative example is a clover-shaped alumina carrier with a diameter of 3 mm and a specific surface area of 98 m 2 / g, water absorption rate is 56%, and the crystal form is γ-Al2O3 and δ-Al2O3.
[0111] Preparation steps of hydrotreating catalyst:
[0112] (1) First, prepare 96 ml of a 0.2 wt% potassium hydroxide solution;
[0113] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to perform atomization pre-spraying treatment on the carrier for 10 minutes. After the pre-spraying, age it for 21 minutes;
[0114] (3) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 6) to prepare 543 ml of active component impregnation solution;
[0115] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 6 hours, dried at 100° C. for 4 hours, and calcined at 520° C. for 5 hours to obtain catalyst D3.
[0116] The difference from Example 5 is that the alumina is not in mesh shape and a conventional carrier is used.
[0117] Comparative Example 4
[0118] The carrier used in this comparative example is a mesh-shaped alumina (honeycomb) carrier with a diameter of 15 mm, a height of 10 mm, and a specific surface area of 82 m 2 / g, water absorption rate is 48%, and the crystal forms are γ-Al2O3, δ-Al2O3, and θ-Al2O3.
[0119] Preparation steps of hydrotreating catalyst:
[0120] (1) First, prepare 41 ml of a 0.4 wt% potassium hydroxide solution;
[0121] (2) Weigh 1 kg of the carrier, add it to a rotating drum, and use the prepared potassium hydroxide solution to spray the carrier for pre-spraying for 6.5 minutes. After pre-spraying, age it for 6 minutes, dry it at 110°C for 2 hours, and roast it at 350°C for 4 hours;
[0122] (3) adding ammonium molybdate, nickel nitrate and potassium hydroxide into a composite solvent prepared from ammonia water and deionized water (ammonia water / water = 1 / 4) to prepare 545 ml of an active component impregnation solution;
[0123] (4) The mesh-shaped carrier treated in step (2) was impregnated in the active component impregnation solution of step (3), aged for 5 hours, dried at 110° C. for 4 hours, and calcined at 500° C. for 4 hours to obtain catalyst D4.
[0124] The difference from Example 7 is that after pre-spraying and aging, drying and roasting are carried out, and then the next step of active component impregnation is carried out.
[0125] The mass contents of the components in the catalysts prepared in Examples 1 to 7 and Comparative Examples 1 to 4 are shown in Table 1 below.
[0126] Table 1 Mass content of each component in the catalyst
[0127]
[0128]
[0129] The catalyst was analyzed by SEM to characterize the distribution of active components on the catalyst. The content of active components at different positions in the catalyst is shown in Table 2 below.
[0130] Table 2 The percentage of active component metal content in different positions of the catalyst to the total content of active components (%)
[0131] Center to 1 / 4 radius 1 / 4 to 1 / 2 radius 1 / 2 to 3 / 4 radius 3 / 4 radius to surface Example 1 1.7 8.7 8.2 81.4 Example 2 3.1 9.8 7.9 79.2 Example 3 2.4 5.9 13.7 78 Example 4 2.2 7.8 11.2 78.8 Example 5 2.6 7.4 12.5 77.5 Example 6 2 8.2 14.6 75.2 Example 7 1.9 10.1 9.4 78.6 Comparative Example 1 6.1 13.7 23.7 56.5 Comparative Example 2 5.5 12.4 30.4 51.7 Comparative Example 3 6.9 14.1 28.9 50.1 Comparative Example 4 5.1 15.5 21.5 57.9
[0132] From the data in Table 2 and Figure 2It can be seen that the active components of the catalyst of the present invention form a gradient distribution, and the surface active components are dispersed more efficiently and more evenly, which is beneficial to the subsequent sulfurization treatment and hydrofining reaction.
[0133] Test Example 1
[0134] Protective agent evaluation:
[0135] The first stage hydrogenation product of pyrolysis gasoline was used as the feedstock oil. The properties of the feedstock oil are shown in Table 3. The C1, C2 and D1, D2 catalysts were compared and evaluated over a long period of 1000 hours. The average data are shown in Table 4 below.
[0136] The catalyst evaluation was carried out on a 500ml adiabatic bed hydrogenation reactor, with 100ml of protective agent loaded on the upper part and 400ml of LY-9802 catalyst loaded on the lower part. Before adding the raw materials to the reaction, the protective agent and catalyst loaded in the reactor were first sulfurized at 280℃ for 10h with naphtha with a CS2 content of 1%, and then cooled to 230℃ to prepare for adding the raw materials. Evaluation process conditions: reaction pressure 2.8MPa, inlet temperature 230~260℃, fresh raw oil volume space velocity: 2.0h -1 , volume ratio of hydrogen to oil: 300:1 (volume ratio based on fresh oil).
[0137] Table 3 Hydrogenation feedstock properties
[0138]
[0139] Table 4 Average data of catalyst evaluation
[0140]
[0141] From the comparison between the above embodiments and the comparative examples, it can be seen that the catalyst prepared by the present invention has relatively low bromine value and total sulfur of the hydrogenation product under the same evaluation process conditions, which fully demonstrates that the protective agent prepared in the embodiment has certain hydrogenation activity and selectivity, and can effectively protect the hydrogenation main catalyst and prolong the service life of the main catalyst.
[0142] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A hydrorefining catalyst, comprising a carrier, an active component and a promoter, wherein the active component comprises molybdenum and nickel, It is characterized in that The carrier comprises mesh-shaped alumina, and the auxiliary agent is potassium, a part of the potassium is introduced in the form of carrier pre-spraying, and a part of the potassium is introduced in the form of active component impregnation liquid. The carrier after pre-spraying needs to be aged and then impregnated with the active component impregnation liquid; the pre-spraying completion time is 1min~20min; potassium hydroxide solution is used in the carrier pre-spraying process.
2. The hydrotreating catalyst according to claim 1, It is characterized in that Based on the total weight of the hydrorefining catalyst being 100%, based on the weight of the corresponding oxide, the content of the active component is 5% to 15%, and the content of the auxiliary agent is 0.01% to 3%.
3. The hydrotreating catalyst according to claim 1, It is characterized in that Based on the total weight of the hydrorefining catalyst being 100%, the content of the additive is 0.1% to 1.5% based on the weight of the corresponding oxide.
4. The hydrotreating catalyst according to claim 1, It is characterized in that The mesh-shaped alumina is cylindrical, with a diameter of 10-20 mm and a height of 5-15 mm.
5. The hydrotreating catalyst according to claim 1, It is characterized in that The mesh-shaped alumina is in a honeycomb shape.
6. The hydrotreating catalyst according to claim 1, It is characterized in that The alumina content in the carrier is ≥80%, and the alumina crystal type includes θ-Al 2 O 3 ,γ-Al 2 O 3 、α-Al 2 O 3 ,δ-Al 2 O 3 At least two of the .
7. The hydrotreating catalyst according to claim 1, It is characterized in that The water absorption rate of the carrier is 35 wt % to 65 wt %.
8. The hydrotreating catalyst according to claim 1, It is characterized in that The water absorption rate of the carrier is 50 wt % to 60 wt %.
9. The hydrotreating catalyst according to claim 1, It is characterized in that The pre-spraying completion time is 3min~10min.
10. The hydrotreating catalyst according to claim 1, It is characterized in that The concentration of the potassium hydroxide solution is 0.1 wt%~5 wt%; the dosage of the potassium hydroxide solution is: 1%X×T ml~20%X×T ml, wherein X represents the water absorption rate of the carrier, and T is the grams of the pre-sprayed carrier.
11. The hydrotreating catalyst according to claim 1, It is characterized in that The concentration of the potassium hydroxide solution is 0.5 wt %~1 wt %, and the dosage of the potassium hydroxide solution is 5%X×T ml~10%X×T ml, wherein X represents the water absorption rate of the carrier, and T is the grams of the pre-sprayed carrier.
12. The hydrotreating catalyst according to claim 1, It is characterized in that The aging time is 5 min to 30 min.
13. The hydrotreating catalyst according to claim 1, It is characterized in that The aging time is 10 min to 20 min.
14. The hydrotreating catalyst according to claim 1, It is characterized in that The volume of the active component impregnation solution is 1.05×(1-the percentage of potassium hydroxide solution added)X×T ml~1.25×(1-the percentage of potassium hydroxide solution added)X×T ml, wherein X represents the water absorption rate of the carrier, and T represents the grams of the pre-sprayed carrier; the active component molybdenum is added to the active component impregnation solution in the form of ammonium molybdate, and the active component nickel is added to the active component impregnation solution in the form of sulfate, halide, nitrate or acetate.
15. The hydrotreating catalyst according to claim 1, It is characterized in that The volume of the active component impregnation solution is 1.10×(1-the percentage of potassium hydroxide solution added)X×T ml~1.20×(1-the percentage of potassium hydroxide solution added)X×T ml, wherein X represents the water absorption rate of the carrier, and T is the weight of the pre-sprayed carrier; the active component nickel is added to the active component impregnation solution in the form of nitrate and / or acetate.
16. A method for preparing the hydrotreating catalyst according to any one of claims 1 to 15, It is characterized in that The following steps are involved: (1) Pre-spray and age the carrier with potassium hydroxide solution. (2) preparing an active ingredient impregnation solution containing potassium; (3) The aged carrier is immersed in the active component impregnation solution, and then aged, dried and calcined.
17. The method for preparing the hydrotreating catalyst according to claim 16, It is characterized in that The drying conditions are: temperature 80-120° C., time 2-6 hours, and the calcination conditions are: temperature 350-600° C., time 3-8 hours.