A metal porous thermally conductive catalyst system and a method for preparing glycolide at low temperature and pressure

Through the method of loading catalysts in porous metal thermally conductive particles, the problems of poor thermal conductivity of oligomers and polymerization at high temperatures are solved, and efficient low-temperature and low-pressure preparation of glycolide is achieved, which improves the yield and purity, and reduces the cost and coking rate. .

CN116212950BActive Publication Date: 2024-10-18WISON ENG

Patent Information

Application Number
CN202111459704.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-02
Publication Date
2024-10-18
Estimated Expiration
2041-12-02

AI Technical Summary

Technical Problem

In the existing technology, oligomers have poor thermal conductivity and are prone to polymerization at high temperatures to form high polymers, resulting in a reduction in glycolide yield. In addition, traditional catalysts are costly and prone to deactivation, causing coking problems.

Method used

Using a metal porous thermally conductive catalyst system, by loading the catalyst in porous metal thermally conductive particles, the thermal conductivity and catalytic activity are improved, the reaction temperature is reduced, the coking rate is reduced, and glycolide is prepared at low temperature and low pressure.

Benefits of technology

The yield and purity of glycolide are improved, the reaction temperature and time are reduced, the coking rate is reduced, the catalyst can be reused, the production cost is reduced, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of chemical products, and specifically to a metal porous thermally conductive catalyst system and a method for preparing glycolide at low temperature and low pressure. The metal porous thermally conductive catalyst system comprises porous metal thermally conductive particles and a catalyst; the catalyst is loaded in the pores of the porous metal thermally conductive particles. The method for preparing glycolide at low temperature and low pressure comprises mixing glycolic acid oligomers with the metal porous thermally conductive catalyst system as described above in the present invention to carry out a depolymerization reaction to prepare glycolide. The present invention designs a porous thermally conductive catalyst, and utilizes the excellent thermal conductivity, dispersibility and porous modifiability of porous metal particles to simultaneously play the three roles of a thermal conductor, a dispersant and a catalyst during the reaction process, so as to achieve a high-efficiency catalyst to reduce the reaction temperature, improve the reaction efficiency, reduce the coking rate and thus increase the glycolide yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical products, and in particular to a metal porous heat-conducting catalyst system and a method for preparing glycolide at low temperature and pressure. Background Art

[0002] Biodegradable materials have attracted much attention in the context of green environmental protection. Polyglycolic acid (PGA) is a widely used biodegradable material with excellent biocompatibility, machinability and gas barrier properties. It is widely used in the fields of biomedicine and packaging materials. At present, the industrial methods for preparing PGA mainly use the direct polymerization of glycolic acid and the ring-opening polymerization of glycolide.

[0003] The direct polymerization method is that the glycolic acid molecules are continuously dehydrated to promote the continuous growth of the molecular chain of the reaction product, but the PGA obtained by this method has a low molecular weight and uneven distribution, and has no practical industrial application value. The ring-opening polymerization method is a commonly used synthesis method for preparing high-molecular PGA in the industry, also known as the two-step method: first, glycolic acid is directly condensed and dehydrated to form glycolic acid oligomers with low molecular weight, and then it is depolymerized under high temperature and high pressure to obtain high-molecular weight PGA polymers. The process is as follows:

[0004] Step 1:

[0005]

[0006] Step 2:

[0007]

[0008] The method of depolymerizing oligomers to produce glycolide mainly uses bulk depolymerization in industry, where oligomers are crushed and melted, and then a catalyst is added to depolymerize under high temperature and reduced pressure to produce glycolide products. Japanese Kureha Patent (CN101606907) reports a method for preparing glycolide, which uses high-purity glycolic acid crystals as raw materials, and obtains high-purity and high-yield glycolide through polycondensation, high-temperature depolymerization, recrystallization and other steps. Liu Cuijuan et al. used ultrasonic catalysis to depolymerize and obtained a crude glycolide product with a yield of 71.2%. The bulk depolymerization process is simple, but there are the following three problems: (1) The oligomers themselves have poor thermal conductivity, and the heat is uneven inside and outside the reactor, which hinders the depolymerization of the reactants inside the system; (2) The oligomers are easy to continue to polymerize to form polymers at high temperatures, producing residues such as block coke; (3) The traditional catalyst in the depolymerization reaction is a solid powder, which is disposable, has a high cost, and is easily coated by coke and loses its activity, and has a higher requirement for the reaction temperature. The above points are not conducive to the depolymerization of oligomers, and are likely to cause coking at the bottom of the kettle, clogging of pipelines and other problems, resulting in a decrease in the yield of glycolide. Therefore, in order to find an efficient catalytic system, enhance the internal thermal conductivity of the system, improve the dispersion of reactants, increase catalytic activity, reduce the reaction temperature, and establish a low-temperature, efficient and low-coking reaction system, which is the main difficulty in synthesizing glycolide. Summary of the invention

[0009] In view of the shortcomings of the prior art described above, the purpose of the present invention is to provide a metal porous thermally conductive catalyst system and a method for preparing glycolide at low temperature and low pressure. In the process of catalytic decomposition of glycolic acid oligomers, a high-efficiency catalyst is selected to lower the reaction temperature, improve the reaction efficiency, reduce the coking rate and thus increase the glycolide yield, thereby solving the problems in the prior art.

[0010] The present invention is achieved through the following technical solutions:

[0011] On the one hand, the present invention provides a metal porous thermally conductive catalyst system for preparing glycolide, wherein the metal porous thermally conductive catalyst system comprises porous metal thermally conductive particles and a catalyst; the catalyst is loaded in the pores of the porous metal thermally conductive particles; and the mass ratio of the porous metal thermally conductive particles to the catalyst is 100:10 to 100:80.

[0012] Another aspect of the present invention provides use of the metal porous thermally conductive catalyst system according to the present invention in the preparation of glycolide.

[0013] Another aspect of the present invention provides a method for preparing glycolide at low temperature and low pressure, comprising mixing glycolic acid oligomers with the aforementioned metal porous thermally conductive catalyst system of the present invention to carry out a depolymerization reaction to prepare glycolide.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] The metal porous thermally conductive catalyst system of the present invention, firstly, utilizes its characteristic of having a relatively high porosity, which is beneficial to improving the distribution density of catalytic active sites and the mass transfer capacity of the catalyst; secondly, utilizes the high thermal conductivity of the metal to improve the heat transfer capacity of the molten oligomers in the depolymerization reaction, promotes the system to be heated evenly, and is beneficial to promoting the efficient and stable progress of the reaction, so that the product glycolide can be continuously and stably evaporated; finally, utilizes the characteristic of the small size of the porous metal, which is helpful to disperse the molten oligomers and effectively improve the formation of polymers during the depolymerization process, thereby solving the coking problem at the bottom of the reactor. In the depolymerization process, the thermal conductivity of the metal porous thermally conductive catalyst system is beneficial to lowering the reaction temperature, reducing the generation of heavy residues, shortening the reaction time, and improving the reaction efficiency. The metal porous thermally conductive catalyst system designed and synthesized by the present invention can be reused many times, is green and environmentally friendly, reduces costs, and is beneficial to large-scale production. DETAILED DESCRIPTION

[0016] The following describes in detail the embodiments of the metal porous thermally conductive catalyst system and the method for preparing glycolide at low temperature and pressure.

[0017] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0018] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0019] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0020] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0021] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0022] The applicant of the present invention has accidentally discovered a metal porous heat-conducting catalyst system through a large number of experiments. In the process of catalytic depolymerization of glycolic acid oligomers, the metal porous heat-conducting catalyst system is selected to reduce the reaction temperature, and the depolymerization reaction of glycolic acid oligomers can be achieved at low temperature, which can improve the reaction efficiency, reduce the coking rate and thus increase the glycolide yield. And on this basis, the present invention was completed.

[0023] On the one hand, the present invention provides a metal porous thermally conductive catalyst system, which includes porous metal thermally conductive particles and a catalyst; the catalyst is loaded in the pores of the porous metal thermally conductive particles. The loading rate of the catalyst can be 10% to 30%, 10% to 20%, 20% to 30%, 10% to 15%, 15% to 20%, 20% to 25%, or 25% to 30%, etc. The catalytically active components are fully compounded with the porous metal particles. The porous structure of the porous metal particles as a carrier increases the contact area between the catalytically active components and the reactants, which is conducive to improving the catalytic activity and allowing the reaction to be carried out at a lower temperature; the catalyst is immobilized in the porous metal thermally conductive particles, is not easy to lose, and the cost is greatly reduced. And the metal porous thermally conductive catalyst system, using the excellent thermal conductivity, dispersibility and porous modifiability of the porous metal particles, simultaneously plays the three roles of thermal conductor, dispersant and catalyst in the reaction process, achieving efficient catalytic depolymerization of polyglycolic acid oligomers, reducing the coking rate and improving the yield.

[0024] Typically, the preparation of a porous metal thermally conductive catalyst system is carried out by placing porous metal thermally conductive particles and a catalyst into a reactor and stirring them at room temperature, for example, by mechanical stirring, so that the catalyst is fully loaded into the pores of the metal thermally conductive particles to obtain a porous metal thermally conductive catalyst system with uniformly dispersed catalytic active sites.

[0025] In the metal porous thermally conductive catalyst system provided by the present invention, the amount of porous metal thermally conductive particles and catalysts needs to meet a certain ratio to achieve full loading. In some embodiments, the mass ratio of the porous metal thermally conductive particles to the catalyst can be, for example, 100:10 to 100:80, 100:10 to 100:30, 100:30 to 100:80, 100:10 to 100:20, 100:20 to 100:30, 100:30 to 100:40, 100:40 to 100:50, 100:50 to 100:60, 100:60 to 100:70, or 100:70 to 100:80, etc. In a specific embodiment, the mass ratio of the porous metal thermally conductive particles to the catalyst is 100:30.

[0026] In the metal porous thermally conductive catalyst system provided by the present invention, the metal of the porous metal thermally conductive particles is selected from one or more combinations of Al, Mg, Fe, Co, Ni, Cu, Zn, Ti, etc.; preferably, the metal of the porous metal thermally conductive particles is selected from one of Fe, Co, Ni, Cu, Zn, etc.

[0027] In the metal porous thermally conductive catalyst system for preparing glycolide provided by the present invention, the porosity of the porous metal thermally conductive particles is 95% to 98%, 95% to 96%, 96% to 97%, or 97% to 98%, etc.; preferably 98%. The volume density of the porous metal thermally conductive particles is 0.5 to 0.9 g / cm 3 , 0.5~0.7g / cm 3 , 0.7~0.9g / cm 3 , 0.5~0.6g / cm 3 , 0.6~0.7 g / cm 3 , 0.7~0.8g / cm 3 , or 0.8~0.9g / cm 3 etc.; preferably 0.7g / cm 3 . The pore size of the porous metal thermally conductive particles can be 0.2-0.4 mm, 0.4-0.7 mm, 0.2-0.3 mm, 0.3-0.4 mm, 0.4-0.5 mm, 0.5-0.6 mm, or 0.6-0.7 mm, etc.; preferably 0.2 mm. The diameter of the porous metal thermally conductive particles can be 1-3 mm, 1-2 mm, or 2-3 mm, etc.; preferably 2 mm. The porous metal particles have high thermal conductivity and can be used as a heat-conducting medium to promote the catalytic depolymerization of glycolic acid oligomers so that the entire system is heated evenly; small-sized metal particles with a diameter of about 1 to 3 mm can be used as dispersants to hinder the further polymerization of oligomers under high temperature conditions, which is beneficial to reduce the coking rate and increase the glycolide yield.

[0028] In the metal porous thermally conductive catalyst system provided by the present invention, the catalyst is selected from one or more combinations of stannous octoate, stannous chloride, tin oxide, zinc oxide, magnesium oxide, titanium dioxide, bismuth oxide, iron acetylacetonate, zinc acetylacetonate, etc.

[0029] Another aspect of the present invention provides use of the metal porous thermally conductive catalyst system according to the present invention in the preparation of glycolide.

[0030] Another aspect of the present invention provides a method for preparing glycolide at low temperature and low pressure, comprising mixing glycolic acid oligomers with the metal porous thermally conductive catalyst system described in the first aspect of the present invention to carry out a depolymerization reaction to prepare glycolide. Specifically, glycolic acid oligomer powder and the metal porous thermally conductive catalyst system can be added to a reaction kettle, the temperature can be further increased, and the depolymerization reaction can be carried out under reduced pressure. During the reaction process, a light yellow liquid is continuously evaporated under the catalysis of the metal porous thermally conductive catalyst system, which is the product glycolide.

[0031] In the method for preparing glycolide at low temperature and low pressure provided by the present invention, the glycolic acid oligomer and the metal porous thermally conductive catalyst system need to react at a suitable ratio. In some embodiments, the mass ratio of the glycolic acid oligomer to the metal porous thermally conductive catalyst system is 100:5-100:80, 100:5-100:20, 100:20-100:80, 100:5-100: 10, 100:10-100:20, 100:20-100:30, 100:30-100:40, 100:40-100:50, 100: 50-100:60, 100:60-100:70, or 100:70-100:80, etc. Preferably, the mass ratio of the glycolic acid oligomer to the metal porous thermally conductive catalyst system is 100:20-80. More preferably, the mass ratio of the glycolic acid oligomer to the metal porous thermally conductive catalyst system is 100:65.

[0032] In the method for preparing glycolide at low temperature and low pressure provided by the present invention, the temperature of the depolymerization reaction may be 190-250°C. The temperature of the depolymerization reaction may be 190-210°C, 210-240°C, 240-250°C, 220-230°C, 230-240°C, or 240-250°C. The temperature of the depolymerization reaction. Preferably, it is 210-240°C; more preferably, it is 220-230°C. The pressure of the depolymerization reaction may be 0.01-10kPa, 0.01-1kPa, 1-3kPa, 3-5kPa, 5-8kPa, or 8-10kPa. The pressure of the depolymerization reaction is preferably 1-3kPa, more preferably 1-1.5kPa. The reaction time of the depolymerization may be 0.1-5h, 0.1-1h, 1-2h, 2-3h, 3-4h, or 4-5h. Under the action of the metal porous thermally conductive catalyst system, the depolymerization reaction temperature is reduced from the current common 250°C to 210-230°C, or even lower, and the reaction pressure is controlled within the range of 1-3kPa, and the reactants are completely depolymerized within 1-3 hours. The metal porous thermally conductive catalyst system uses the excellent thermal conductivity, dispersibility and porous modifiability of porous metal particles to simultaneously act as a thermal conductor, dispersant and catalyst during the reaction process, achieving efficient catalytic depolymerization of polyglycolic acid oligomers, while reducing the coking rate and increasing the yield of glycolide, and reducing costs.

[0033] Beneficial effects of the present invention:

[0034] The metal porous thermally conductive catalyst system of the present invention, firstly, utilizes its characteristic of having a relatively high porosity, which is beneficial to improving the distribution density of catalytic active sites and the mass transfer capacity of the catalyst; secondly, utilizes the high thermal conductivity of the metal to improve the heat transfer capacity of the molten oligomers in the depolymerization reaction, promotes the system to be heated evenly, and is beneficial to promoting the efficient and stable progress of the reaction, so that the product glycolide can be continuously and stably evaporated; finally, utilizes the characteristic of the small size of the porous metal, which is helpful to disperse the molten oligomers and effectively improve the formation of polymers during the depolymerization process, thereby solving the coking problem at the bottom of the reactor. In the depolymerization process, the thermal conductivity of the metal porous thermally conductive catalyst system is beneficial to lowering the reaction temperature, reducing the generation of heavy residues, shortening the reaction time, and improving the reaction efficiency. The metal porous thermally conductive catalyst system designed and synthesized by the present invention can be reused many times, is green and environmentally friendly, reduces costs, and is beneficial to large-scale production.

[0035] The yield of glycolide prepared by the invention is as high as 96%, the purity is as high as 95%, and the reaction coking rate can be as low as 1.9%.

[0036] The beneficial effects of the present invention are further illustrated below in conjunction with embodiments.

[0037] In order to make the invention purpose, technical scheme and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with examples. However, it should be understood that the examples of the present invention are only for explaining the present invention, not for limiting the present invention, and the examples of the present invention are not limited to the examples given in the specification. The specific experimental conditions or operating conditions not specified in the examples are made under conventional conditions, or are made under the conditions recommended by the material supplier.

[0038] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0039] In the following examples, the reagents, materials and instruments used are all commercially available unless otherwise specified.

[0040] Embodiment 1:

[0041] A method for efficiently preparing glycolide, comprising the following steps:

[0042] Weigh 100g of porous Fe particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 10g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 90%, the purity is 94%, and the reaction coking rate is 6.1%.

[0043] Embodiment 2:

[0044] A method for efficiently preparing glycolide, comprising the following steps:

[0045] Weigh 100g of porous Co small particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 10g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 89%, the purity is 90%, and the reaction coking rate is 5.3%.

[0046] Embodiment 3:

[0047] A method for efficiently preparing glycolide, comprising the following steps:

[0048] Weigh 100g of porous Ni small particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 10g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 86%, the purity is 95%, and the reaction coking rate is 7.9%.

[0049] Embodiment 4:

[0050] A method for efficiently preparing glycolide, comprising the following steps:

[0051] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3, pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 10g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 92%, the purity is 93%, and the reaction coking rate is 4.4%.

[0052] Embodiment 5:

[0053] A method for efficiently preparing glycolide, comprising the following steps:

[0054] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 20g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 95%, the purity is 95%, and the reaction coking rate is 3.7%.

[0055] Embodiment 6:

[0056] A method for efficiently preparing glycolide, comprising the following steps:

[0057] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 2h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 96%, the purity is 95%, and the reaction coking rate is 1.9%.

[0058] Embodiment 7:

[0059] A method for efficiently preparing glycolide, comprising the following steps:

[0060] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked flask equipped with a condenser, a stirring device and a decompression device, add 30g of bismuth oxide, stir at room temperature for 30min to allow bismuth oxide to fully fill the pores of the thermally conductive particles, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked flask, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 90%, the purity is 92%, and the reaction coking rate is 4.9%.

[0061] Embodiment 8:

[0062] A method for efficiently preparing glycolide, comprising the following steps:

[0063] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked flask equipped with a condensing device, a stirring device and a decompression device, add 30g of stannous chloride, stir at room temperature for 30min to make the stannous chloride fully fill the pores of the thermally conductive particles to form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked flask, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 88%, the purity is 91%, and the reaction coking rate is 7.1%.

[0064] Embodiment 9:

[0065] A method for efficiently preparing glycolide, comprising the following steps:

[0066] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3, pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 240°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 90%, the purity is 94%, and the reaction coking rate is 3.2%.

[0067] Embodiment 10:

[0068] A method for efficiently preparing glycolide, comprising the following steps:

[0069] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 190°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 5h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 83%, the purity is 90%, and the reaction coking rate is 3.8%.

[0070] Embodiment 11:

[0071] A method for efficiently preparing glycolide, comprising the following steps:

[0072] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 200°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 4h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 87%, the purity is 94%, and the reaction coking rate is 4.9%.

[0073] Embodiment 12:

[0074] A method for efficiently preparing glycolide, comprising the following steps:

[0075] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 4kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 90%, the purity is 94%, and the reaction coking rate is 5.4%.

[0076] Embodiment 13:

[0077] A method for efficiently preparing glycolide, comprising the following steps:

[0078] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 7kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 4h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 88%, the purity is 95%, and the reaction coking rate is 5.9%.

[0079] Embodiment 14:

[0080] A method for efficiently preparing glycolide, comprising the following steps:

[0081] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3, pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 10kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 5h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 86%, the purity is 96%, and the reaction coking rate is 6.1%.

[0082] Embodiment 15:

[0083] A method for efficiently preparing glycolide, comprising the following steps:

[0084] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 430g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 4h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 88%, the purity is 91%, and the reaction coking rate is 3.3%.

[0085] Embodiment 16:

[0086] A method for efficiently preparing glycolide, comprising the following steps:

[0087] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 165g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 92%, the purity is 91%, and the reaction coking rate is 2.1%.

[0088] Embodiment 17:

[0089] A method for efficiently preparing glycolide, comprising the following steps:

[0090] Weigh 100g of porous Cu particles (porosity 98%, pore volume 0.7g / cm 3 , pore size 0.2mm, diameter 2mm) in a three-necked bottle with a condensing device, a stirring device and a decompression device, add 30g of stannous octoate, stir at room temperature for 30min to allow the pores of the thermally conductive particles to fully adsorb stannous octoate, and form a metal porous thermally conductive catalyst system. Continue to add 200g of glycolic acid oligomer powder with a weight average molecular weight of 40,000 to the three-necked bottle, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 3h, indicating that the reaction is over. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 90%, the purity is 92%, and the reaction coking rate is 2.6%.

[0091] Comparative Example 1:

[0092] The blank comparison experiment includes the following steps:

[0093] Add 200g of glycolic acid oligomer powder with a weight average molecular weight of 20,000 to a three-necked flask, quickly heat the reaction to 230°C, control the system pressure to 1kPa, and light yellow liquid glycolide evaporates during the reaction. No product evaporates after 6 hours, indicating that the reaction is complete. After cooling, a light yellow solid is obtained, which is glycolide. The glycolide yield is 76%, the purity is 90%, and the reaction coking rate is 14.7%.

[0094] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A metal porous thermally conductive catalyst system for preparing glycolide at low temperature and low pressure, the metal porous thermally conductive catalyst system comprising porous metal thermally conductive particles and a catalyst; the catalyst is loaded in the pores of the porous metal thermally conductive particles; the porous metal thermally conductive particles have a porosity of 95% to 98% and a volume density of 0.5 to 0.9 g / cm 3 The pore size is 0.2-0.7 mm and the diameter is 1-3 mm; the mass ratio of the porous metal thermally conductive particles to the catalyst is 100:10-100:80; the metal porous thermally conductive catalyst system is used for catalytic depolymerization of glycolic acid oligomers with a weight average molecular weight of 20,000-40,000 to prepare glycolide, and the catalyst is selected from one or a combination of stannous octoate and bismuth oxide.

2. The porous metal thermally conductive catalyst system according to claim 1, characterized in that: The metal of the porous metal thermally conductive particles is selected from one or more combinations of Al, Mg, Fe, Co, Ni, Cu, Zn, and Ti.

3. The metal porous thermally conductive catalyst system according to claim 2, characterized in that: The metal of the porous metal thermally conductive particles is selected from one of Fe, Co, Ni, Cu and Zn.

4. Use of the metal porous thermally conductive catalyst system according to any one of claims 1 to 3 in the preparation of glycolide.

5. A method for preparing glycolide at low temperature and low pressure, comprising mixing glycolic acid oligomers with the metal porous thermally conductive catalyst system according to any one of claims 1 to 3 to carry out a depolymerization reaction to prepare glycolide.

6. The method for preparing glycolide at low temperature and low pressure according to claim 5, characterized in that: The mass ratio of the glycolic acid oligomer to the metal porous thermal conductive catalyst system is 100:5-100:

80.

7. The method for preparing glycolide at low temperature and low pressure according to claim 6, characterized in that: The mass ratio of the glycolic acid oligomer to the metal porous thermal conductive catalyst system is 100:20-80.

8. The method for preparing glycolide at low temperature and low pressure as claimed in claim 5, characterized in that: The temperature of the depolymerization reaction is 190-350°C.

9. The method for preparing glycolide at low temperature and low pressure according to claim 8, characterized in that: The temperature of the depolymerization reaction is 210-240°C.

10. The method for preparing glycolide at low temperature and low pressure according to claim 9, characterized in that: The temperature of the depolymerization reaction is 220-230°C.

11. The method for preparing glycolide at low temperature and low pressure according to claim 5, characterized in that: The pressure of the depolymerization reaction is 0.01-10 kPa; And / or, the reaction time of the depolymerization is 0.1 to 5 h.

12. The method for preparing glycolide at low temperature and low pressure according to claim 11, characterized in that: The pressure of the depolymerization reaction is 1-3 kPa.

13. The method for preparing glycolide at low temperature and low pressure according to claim 11, characterized in that: The pressure of the depolymerization reaction is 1-1.5 kPa.

14. The method for preparing glycolide at low temperature and low pressure according to claim 5, characterized in that: The weight average molecular weight of the glycolic acid oligomer is 20,000-30,000.

Citation Information

Patent Citations

  • Low-temperature high-efficiency glycolide preparation method based on catalytic depolymerization

    CN104163810A

  • Glycolide as well as preparation method and application thereof

    CN112707884A

Cited By

  • High-thermal-conductivity core-shell copper-zinc-aluminum catalyst, preparation method thereof and application of catalyst in methanol reforming hydrogen production reaction

    CN120586941A