Preparation method and application of ellipsoidal niobium triselenide

By simplifying the process through DC arc plasma discharge, ellipsoidal Nb2Se3 can be synthesized at low cost, solving the problems of long preparation time and high cost in existing technologies. This achieves efficient and environmentally friendly Nb2Se3 preparation and electrocatalytic activity.

CN116216656BActive Publication Date: 2024-11-08JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310125554.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-16
Publication Date
2024-11-08
Estimated Expiration
2043-02-16

AI Technical Summary

Technical Problem

Existing methods for synthesizing sesquichalcogenides are time-consuming, cumbersome, costly, and have poor reproducibility. They also easily introduce impurities, making it difficult to achieve efficient, economical, and environmentally friendly Nb2Se3 preparation.

Method used

By employing a DC arc plasma discharge method, niobium and selenium are discharged in a ratio lower than the stoichiometric ratio after tableting to directly synthesize ellipsoidal Nb2Se3. This method simplifies the process, reduces raw material consumption, and is both environmentally friendly and efficient.

Benefits of technology

A high-yield, low-cost, and stable Nb2Se3 preparation method was achieved, which exhibits good electrocatalytic activity and is suitable as a catalyst for hydrogen evolution reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116216656B_ABST
    Figure CN116216656B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method and application of ellipsoidal niobium triselenide. Niobium powder and selenium powder are uniformly mixed in a molar ratio of 0.2:1-0.5:1, pressed into sheets, and placed between the horizontally placed cathode and anode in a DC arc plasma discharge device. Under the protection of a water cooling system and an argon atmosphere, the gas pressure is raised to 20-60 kPa and the reaction current is 120-140 A. Arc discharge is initiated at the cathode and cathode, and the powder is cooled and passivated to room temperature after the reaction is complete. A gray-black powder is collected in a graphite pot, and its microscopic morphology is ellipsoidal Nb2Se3 with a major axis range of 0.5-2 μm. The niobium selenide material containing the ellipsoidal Nb2Se3 is used as a catalyst for the hydrogen evolution reaction at 5 mV·s ‑1 At a scan rate of 10 mA cm ‑2 An overpotential of 304 mV can be achieved at a current density of , indicating that the niobium selenide material containing ellipsoidal Nb2Se3 has a certain catalytic activity for hydrogen evolution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic nano material preparation, and specifically relates to a preparation method and application of ellipsoidal niobium triselenide as a hydrogen evolution reaction (HER) catalyst. Background Art

[0002] Transition metal chalcogenides have attracted widespread attention in recent years due to their rich optical and electrical properties and broad application prospects in catalysis, electronics and energy storage. Transition metal chalcogenides AB2 (A represents transition metal elements, B represents S, Se and other elements) have quasi-two-dimensional layered structures and high electrocatalytic hydrogen evolution activity. They can currently replace precious metal platinum (Pt) as high-efficiency HER electrocatalyst candidate materials. However, some molybdenum and niobium sulfides and selenides have received relatively little attention, such as chalcogenides with chemical composition A:B=2:3 (A=Mo, Nb; B=S, Se). Chalcogenides with this stoichiometric Mo or Nb are called sesquichalcogenides. Researchers predict that sesquichalcogenides (such as Nb2Se3, Mo2S3) can add more metal centers to this structural unit, thereby producing new electrocatalytic HER candidate materials.

[0003] At present, the methods for synthesizing sesquichalcogenides mainly include chemical vapor deposition and vacuum solid phase sintering. Ivanova (Physical Chemistry Chemical Physics, 21, 2019, 1454) et al. used vacuum solid phase sintering to place equal amounts of Mo and S precursors in a vacuum quartz ampoule, first heat-treating the precursors at 600°C for 3 hours, and then further heating to 1100°C for 72 hours to obtain Mo2S3; placing equal amounts of Nb and Se precursors in a vacuum quartz tube, keeping them at 1100°C for 90 hours, and obtaining Nb2Se3 by quenching and cooling the quartz tube in an ice water bath. This method requires pretreatment of the raw materials, and the preparation of Mo2S3 and Nb2Se3 materials takes a long time, the operation is cumbersome, the amount of samples obtained is very limited, and excessive raw materials are consumed. Zhong (Applied Surface Science, 263, 2012, 410) et al. introduced gold particles as nucleation sites by chemical vapor deposition to synthesize high-density three-dimensional Mo2S3 nanoflowers with controlled sites. The preparation process of this method introduced gold particles as nucleation sites, which had an impact on the performance of Mo2S3 nanoflowers. Peng (Applied Physics Letters, 83, 2018, 3561) et al. synthesized uniform Mo2S3 nanorods by solid-phase reaction between porous Al2O3 impregnated with MoO3 and H2S gas. In this preparation process, molybdenum oxide was used as an experimental raw material, which was difficult to avoid introducing a small amount of impurities, and long-term preparation would lead to environmental pollution problems. The above methods for synthesizing sesquisulfide compounds usually use excessive raw materials, or through multi-step reactions, add other auxiliary raw materials to synthesize the desired products, which have the disadvantages of high production cost, complex process, cumbersome preparation, long production cycle, poor repeatability, and low yield. Therefore, from the perspective of economic cost and green environmental protection, it is urgent to develop an economical, fast, efficient and stable synthesis route. The present invention provides a method for preparing a niobium selenide material containing ellipsoidal Nb2Se3 in a one-step process under low niobium conditions, and obtains a product in a wide range of molar ratios of niobium to selenium of 0.2:1-0.5:1. Compared with the traditional method, it reduces unnecessary raw material consumption, greatly reduces production costs, and can be directly used as an electrocatalytic HER active material. Summary of the invention

[0004] The present invention mainly provides a method for preparing ellipsoidal Nb2Se3 in one step, which has the advantages of simple process, low cost, good repeatability and can synthesize Nb2Se3 at a ratio lower than the stoichiometric ratio of 0.2:1-0.5:1 (stoichiometric ratio of 2:3), reduces the cost of raw materials and avoids the waste of raw materials, is environmentally friendly, and the synthesized product has a high yield and can be directly used as a hydrogen evolution electrocatalytic active material.

[0005] The specific operation process of the present invention is as follows:

[0006] 1. Weigh niobium powder and selenium powder in a molar ratio of 0.2:1-0.5:1 and put them into an agate mortar and grind for 30 minutes to evenly mix the niobium powder and selenium powder. Put the ground niobium and selenium mixed powder into a tablet pressing mold and press it into a disc with a height of about 2.5 mm through the process of pressurization, pressure holding and pressure relief.

[0007] 2. Place the pressed sample disc into the anode graphite pot in the horizontal DC arc plasma discharge device. The cathode is a tungsten rod. Adjust the horizontal axis of the cathode tungsten rod and the anode graphite pot to coincide. The distance between the positive and negative poles is about 1 cm.

[0008] 3. Close the reaction device and perform the process of vacuuming-washing-vacuuming at least three times. After washing, the pressure in the device is reduced to below 10Pa. Under the protection of cooling circulating water and argon atmosphere, the pressure in the device is raised to 20-60kPa. Start the arc power supply, set the current to 120-140A, adjust the distance between the positive and negative electrodes to start the arc, and keep the arc stable for 10 minutes until the reaction is complete, and then turn off the power supply of the DC arc welding machine.

[0009] 4. Cool and passivate in a water cooling system and argon atmosphere for 1-3 hours. Gray-black powder containing Nb2Se3 is collected in the anode graphite pot.

[0010] 5. The prepared niobium selenide material containing ellipsoidal Nb2Se3 is directly used as an active material to obtain a hydrogen evolution reaction catalyst with low charge transfer resistance and high electron transfer rate.

[0011] The advantage of the present invention over the prior art is that ellipsoidal Nb2Se3 can be prepared under the condition of less niobium, which greatly reduces the consumption of raw materials. In addition, the preparation process is simple, stable, cost-effective, safe and environmentally friendly, and highly repeatable. Niobium selenide material containing ellipsoidal Nb2Se3 can be obtained in one step and can be directly used as a hydrogen evolution electrocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 Schematic diagram of the structure of DC arc plasma discharge device.

[0013] Figure 2 X-ray diffraction (XRD) patterns of ellipsoidal Nb2Se3 and hexagonal (2H) phase NbSe2.

[0014] Figure 3 Scanning electron microscope (SEM) image of ellipsoidal Nb2Se3.

[0015] Figure 4 Transmission electron microscopy (TEM) image of ellipsoidal Nb2Se3.

[0016] Figure 5 High-resolution transmission electron microscopy (HRTEM) image of ellipsoidal Nb2Se3.

[0017] Figure 6 Linear sweep voltammetric (LSV) curves of ellipsoidal Nb2Se3 and hexagonal (2H) phase NbSe2.

[0018] Figure 7 Tafel plots of ellipsoidal Nb2Se3 and hexagonal (2H) phase NbSe2. DETAILED DESCRIPTION

[0019] Example 1 DC arc plasma discharge device

[0020] Figure 1 This is a schematic diagram of the structure of a DC arc plasma discharge device. The importance of the water cooling system lies in: ① Before the reaction, circulating cooling water is introduced to ensure the safe operation of the equipment. The outer cooling water flows in from the water inlet 2, passes through the entire outer cavity 1, and flows out from the water outlet 3; the inner cooling water flows in from the water inlet 5, passes through the inner water cooling sleeve 4, and flows out from the water outlet 6; the anode cooling water flows in from the water inlet 7 and flows out from the water outlet 8. ② During the reaction, the temperature gradient generated between the circulating water cooling zone and the high-temperature arc is a necessary condition for the production of pure NbSe2. ③ After the reaction, the water cooling system plays a role in cooling and passivation.

[0021] Example 2 Preparation process of ellipsoidal Nb2Se3

[0022] Weigh niobium powder and selenium powder according to the molar ratio of 0.2:1-0.5:1 respectively, put them into an agate mortar and grind them for 30 minutes to mix them evenly. Put the ground mixture into the tablet press mold and press it into a cylindrical sheet with a height of 2.5mm and a diameter of 1cm. Put the disc into the horizontally placed anode graphite pot and fix it on one side of the device. The cathode tungsten rod is fixed on the other side of the reaction device, coinciding with the horizontal axis of the anode graphite pot, and the distance between the positive and negative poles is adjusted to about 1cm. Close the reaction device, wash the air repeatedly at least three times, and pump the air pressure in the device to below 10Pa. Raise the air pressure in the device to 20-60kPa under the protection of the water cooling system and argon atmosphere. Start the arc power supply, set the reaction current to 120-140A, and start the arc discharge. The discharge stops after the reaction lasts for 10 minutes. After being cooled and passivated for 3 h to room temperature in a water cooling system and in an argon atmosphere, a gray-black powder containing ellipsoidal Nb2Se3 was collected in the anode graphite pot.

[0023] The prepared ellipsoidal Nb2Se3-containing niobium selenide material was directly used as the active material, acetylene black was used as the conductive agent, PTFE (polytetrafluoroethylene) was used as the binder, and NMP (N-methylpyrrolidone) was used as the solvent. The mixture was mixed at a mass ratio of active material: conductive agent: binder = 8:1:1 and coated on an area of ​​1 cm 2 The carbon cloth was used as the working electrode. The graphite rod was used as the counter electrode, mercury / mercuric oxide was used as the reference electrode, and 0.5M sulfuric acid solution was used as the electrolyte. It was pretreated with hydrogen before the test. -1 Linear sweep voltammetry was performed at a scan rate of 1.5 volts. Electrochemical tests were performed using a Princeton electrochemical workstation.

[0024] Figure 2 The X-ray diffraction (XRD) diagrams of the quasi-ellipsoidal Nb2Se3 and hexagonal (2H) phase NbSe2 obtained in Example 2 are given, and the diffraction peaks in the diagram can match the JCPDS no.21-601 and JCPDS no.87-2415 standard cards. The characteristic peaks of the quasi-ellipsoidal Nb2Se3 are located at 2θ angles of 14.96°, 30.46°, and 49.52°, respectively, corresponding to (-101), (-202), and (-311) crystal planes. It can be seen that the obtained product contains quasi-ellipsoidal Nb2Se3.

[0025] Figure 3 The scanning electron microscope (SEM) image of ellipsoidal Nb2Se3 is given. It can be clearly seen from the image that most of the product Nb2Se3 is ellipsoidal. The long axis range of the ellipsoidal Nb2Se3 is 0.5-2μm.

[0026] Figure 4 This is a transmission electron microscope (TEM) image of ellipsoidal Nb2Se3. The morphology of the ellipsoidal Nb2Se3 in the image is consistent with the SEM result.

[0027] Figure 5 The high-resolution transmission electron microscopy (HRTEM) image of the ellipsoidal Nb2Se3 is given, and the spacing d of the lattice fringes is calculated to be It shows that Nb2Se3 grows along the (-112) crystal plane.

[0028] Figure 6 The linear sweep voltammetric (LSV) curves of ellipsoidal Nb2Se3 and hexagonal (2H) phase NbSe2 show that the niobium selenide material containing ellipsoidal Nb2Se3 has a high current density at -10 mA·cm -2 An overpotential of 304 mV can be achieved at a current density of , indicating that the niobium selenide material containing ellipsoidal Nb2Se3 has a certain catalytic activity for hydrogen evolution.

[0029] Figure 7The Tafel curves of ellipsoidal Nb2Se3 and hexagonal (2H) phase NbSe2 are shown in Figure 1. The Tafel slope in the figure can indicate the quality of electron transfer rate and reveal the mechanism of HER kinetics. As shown in the figure, the Tafel slope of niobium selenide containing ellipsoidal Nb2Se3 is 130mV·dec -1 , indicating that the electron transfer rate in the niobium selenide material containing ellipsoidal Nb2Se3 is faster.

[0030] The embodiments described above only describe the preferred implementation modes of the present invention and do not limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing ellipsoidal niobium triselenide, characterized in that: The main steps are as follows: (1) mixing niobium powder and selenium powder in a molar ratio of 0.2:1-0.5:1 and pressing into tablets; (2) placing the pressed disc between the cathode and cathode in a horizontal DC arc plasma discharge device, with the cathode being a tungsten rod and the anode being a graphite pot; (3) Under the protection of a water cooling system and an inert gas atmosphere, the gas pressure is raised to 20-60 kPa after gas washing, the reaction current is set to 120-140 A, the arc is started until the reaction is complete, and after cooling and passivation to room temperature, a gray-black powder containing Nb2Se3 can be collected in a graphite pot; (4) The prepared niobium selenide material containing ellipsoidal Nb2Se3 is directly used as an active material to obtain a hydrogen evolution reaction catalyst with low charge transfer resistance and high electron transfer rate.

2. The method for preparing ellipsoidal niobium triselenide according to claim 1, characterized in that: During the discharge process, circulating cooling water is introduced into the water cooling system.

3. The method for preparing ellipsoidal niobium triselenide according to claim 1, characterized in that: The purity of niobium powder, selenium powder and inert gas is maintained above 99.99%.

4. Use of a niobium selenide catalyst containing ellipsoidal Nb2Se3 prepared by the preparation method according to any one of claims 1 to 3 in a hydrogen evolution reaction, characterized in that: The niobium selenide hydrogen evolution catalyst containing ellipsoidal Nb2Se3 is directly obtained by using a direct current arc plasma discharge device.