A method for synthesizing nano molecular sieves
By subjecting existing molecular sieves to fluoride treatment and crystal seed-assisted methods, the problems of molecular sieve catalyst deactivation and difficulty in synthesizing nanomolecular sieves are solved, achieving more efficient catalytic performance and service life.
Patent Information
- Application Number
- CN202310143578.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The narrow pore structure of existing molecular sieves leads to channel blockage and catalyst deactivation during the catalytic process, making it difficult to synthesize uniformly dispersed nanomolecular sieves.
By treating the existing molecular sieves with fluoride, part of the crystal skeleton is dissolved, the grain size is reduced and the surface activity is improved. The fluorine-treated molecular sieves are used as seeds, and nanomolecular sieves are synthesized by combining the seed-assisted method.
It significantly improves the molecular sieve's mass transfer, diffusion and anti-coking capabilities, prolongs the service life of the catalyst and optimizes the catalytic performance.
Smart Images

Figure CN116216733B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieve synthesis, and relates to a method for synthesizing a nano molecular sieve by using a molecular sieve treated with fluoride as a seed. Background Art
[0002] Molecular sieve is an important inorganic porous material. It is widely used in the field of catalysis because of its regular pore structure, adjustable acidity and excellent stability. While the regular pore structure of molecular sieve provides it with excellent shape-selective catalytic ability, its narrow pore structure also inhibits the diffusion of macromolecules in the crystal, resulting in rapid blockage of the pores during the catalytic process and ultimately causing catalyst deactivation (Science & Technology in Chemical Industry, 2020, 28 (06), 53-57.). To solve this problem, researchers currently regulate the properties of molecular sieves mainly from two perspectives. On the one hand, using a "top-down" approach, the synthesized molecular sieves are treated with hydrothermal treatment or chemical etching (acid, alkali, fluorine) to introduce a stepped pore structure into the molecular sieve crystal, thereby improving its mass transfer capacity (Chemical Industry and Engineering Progress, 2019, 38 (11), 4965-4970.). On the other hand, in a "bottom-up" manner, either a step-pore molecular sieve with intracrystalline mesopores is prepared, or a nanomolecular sieve is synthesized (Chemical Journal of Chinese Universities, 2022, 43(03), 40-46), or the orientation of the molecular sieve crystals is controlled to prepare a sheet molecular sieve (Petrochemical Technology, 2020, 49(06), 529-537.). In addition, there is also a method of preparing molecular sieves by seed-assisted method and controlling the properties of the seed crystals to control the final product molecular sieve (Natural Gas Chemical Industry, 2015, 32(05), 109-112. Journal of Molecular Catalysis, 2019, 33(02), 113-123.).
[0003] When synthesizing molecular sieves by seed method, the added molecular sieve seeds will act as crystal nuclei to induce new molecular sieves to grow epitaxially along the seeds. Therefore, the size and dispersibility of the seeds will directly affect the grain size and dispersibility of the product molecular sieve. In order to synthesize uniformly dispersed nanomolecular sieves, it is necessary to use uniformly dispersed nanomolecular sieves as seeds. However, the conditions for synthesizing nanomolecular sieves are generally harsh, and highly dispersed nanomolecular sieves are often difficult to obtain. The advantage of the method shown in the present invention is that by subjecting the existing molecular sieves to a certain degree of fluorine treatment and dissolving part of the crystal skeleton by fluorine ion etching, the existing industrial molecular sieves can be directly converted into molecular sieve seeds with uniformly dispersed grains, high crystallinity, and nanometer size. Then, when synthesizing molecular sieves by seed-assisted method, using this fluorine-treated molecular sieve as nanocrystal seeds, nanomolecular sieves can be easily prepared. This method prepares nanocrystal seeds from existing industrial molecular sieves by fluorine etching, avoiding the difficulties faced by direct synthesis of nanomolecular sieves. Summary of the invention
[0004] The present invention aims to provide a method for synthesizing nano molecular sieves using fluoride treated molecular sieves as seed crystals. The size of the zeolite molecular sieve crystal grain size is directly related to the nucleation rate and the growth rate of the crystal. Adding smaller seed crystals to the synthesis system can increase the number of crystal nuclei per unit volume, making the crystallization rate greater than the growth rate of the crystal, which is conducive to the formation of nano molecular sieves, and can effectively reduce the mass transfer and diffusion resistance inside the molecular sieve crystals and improve their mass transfer capacity.
[0005] The present invention firstly uses a concentrated fluoride solution to treat the molecular sieve to be used as a seed crystal, and utilizes the characteristics of being able to simultaneously dissolve the molecular sieve framework silicon and aluminum and preferentially act on the molecular sieve twin interface to disperse the molecular sieve particles, reduce the grain size to half or less of the original size, make the morphology more irregular, and increase the external specific surface area, surface hydroxyl content and surface activity, but retain the crystallinity. Then, the molecular sieve treated with fluorine is used as a seed crystal, and the molecular sieve is synthesized by a seed crystal assisted method.
[0006] To achieve the above object, the present invention discloses a method for synthesizing nanomolecular sieves, comprising the following steps:
[0007] 1) using a fluoride solution to treat the molecular sieve to be used as a seed crystal, so that the molecular sieve particles are evenly dispersed, and the grain size of the molecular sieve after the fluorine treatment is reduced to half or less of the original size;
[0008] 2) Then, the fluorine-treated molecular sieve is used as a seed crystal, and the molecular sieve is synthesized by a seed crystal-assisted method to obtain a nano molecular sieve product;
[0009] The method may or may not use an organic compound structure directing agent and / or a templating agent.
[0010] The fluorine treatment described in step 1) is carried out in a fluorine-containing solution such as hydrogen fluoride, ammonium fluoride, ammonium bifluoride, etc., wherein the mass percentage concentration of fluoride is 5-45wt%, preferably 20-40wt%; the mass ratio of the molecular sieve to be treated to the fluorine-containing solution is 1:1-1:30, the fluorine treatment temperature is 0°C-100°C, and the treatment time is 10min-24h. The treatment process may or may not be assisted by external field enhancement such as ultrasonic treatment; preferably, the grain size of the molecular sieve after fluorine treatment is reduced to 20-50% of the original size, more preferably 30-45%.
[0011] Before the fluorine treatment in step 1), the molecular sieve may be subjected to pretreatment such as ammonium exchange and acid treatment, and then subjected to subsequent fluorine treatment; or the molecular sieve may not be subjected to any pretreatment before the fluorine treatment.
[0012] After the fluorine treatment in step 1), the fluorine ion solution can be filtered and washed to obtain a molecular sieve solid, which is then used as a seed for synthesizing the molecular sieve; or after the fluorine treatment, the solution containing fluorine ions and molecular sieves can be directly used for the subsequent synthesis of molecular sieves without filtering.
[0013] The seed-assisted method described in step 2) is a common molecular sieve synthesis method, in which seed-assisted method completely or partially replaces the organic compound structure directing agent and / or template agent with seed crystals.
[0014] The molecular sieves described in step 1) and step 2) are any molecular sieves synthesized by the seed crystal method, among which molecular sieves with one-dimensional or two-dimensional pore structures such as MOR, TON, FER, and molecular sieves with three-dimensional mesopore and small pore structures such as MFI and MEL are preferred.
[0015] The technical effect of the present invention is that compared with the molecular sieve synthesized by using the original molecular sieve without fluorine treatment as the seed crystal, the molecular sieve synthesized by using the molecular sieve treated with fluoride as the seed crystal has a smaller crystal size, which can improve the mass transfer diffusion capacity and anti-coking ability of the molecular sieve to a greater extent, and extend the service life of the molecular sieve catalyst. The present invention further optimizes the process conditions of fluoride treatment, and significantly enhances the mass transfer diffusion capacity and anti-coking ability of the molecular sieve catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 .a and b are scanning electron microscope images of the molecular sieve before and after fluorine treatment in Example 1, respectively;
[0017] Figure 2 .a and b are scanning electron microscope images of the molecular sieves in Example 1 and Example 2, respectively;
[0018] Figure 3 .a and b are scanning electron microscope images of the molecular sieves in Example 3 and Example 4, respectively;
[0019] Figure 4 .a and b are scanning electron microscope images of the molecular sieves in Example 5 and Example 6, respectively;
[0020] Figure 5 .a and b are scanning electron microscope images of the molecular sieves in Example 7 and Example 8, respectively;
[0021] Figure 6 .a and b are transmission electron microscopy images of the molecular sieves in Example 7 and Example 8, respectively;
[0022] Figure 7 . XRD spectra of Example 1 and Comparative Examples 1, 3, and 5;
[0023] Figure 8 . BET diagrams of Examples 7 and 8;
[0024] Fig. 9 . BET diagrams of Example 1 and Comparative Examples 3 and 5;
[0025] Fig.10 .DME catalytic performance evaluation diagram of Example 1 and Comparative Examples 1, 3, 4;
[0026] Fig.11 .a and b are scanning electron microscope images of comparative example 1 and comparative example 2, respectively. DETAILED DESCRIPTION
[0027] In order to better understand the present invention, the content of the present invention is further illustrated by using specific embodiments below, and the content of the present invention is not limited to the following examples.
[0028] Example 1
[0029] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0030] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0031] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it twice with deionized water;
[0032] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0033] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0034] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0035] 6) preparing 300 g of 30% ammonium fluoride solution, adding 10 g of the sample obtained in step 5), treating with ultrasound at 50° C. for 30 min, taking out the obtained sample, washing it three times by centrifugation, collecting the sample, and drying it in an oven at 100° C. for 24 h. The obtained sample is a nano-molecular sieve seed crystal, and the particle size of the nano-molecular sieve seed crystal is 40% of the particle size before treatment;
[0036] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then adding the nano molecular sieve seed crystals obtained in step 6) in an amount of 10%; stirring continuously for 24 hours to obtain a homogeneous mixture;
[0037] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0038] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 1.
[0039] Example 2
[0040] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0041] 1) 80 g of ammonium chloride was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0042] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it three times with deionized water;
[0043] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0044] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0045] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0046] 6) preparing 300 g of 30% ammonium fluoride solution, adding 10 g of the sample obtained in step 5), treating with ultrasound at 50° C. for 30 min, taking out the obtained sample, washing it five times by centrifugation, collecting the sample, and drying it in an oven at 100° C. for 24 h. The obtained sample is a nano-molecular sieve seed crystal, and the particle size of the nano-molecular sieve seed crystal is 40% of the particle size before treatment;
[0047] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:15.0; then adding the nano molecular sieve seed obtained in step 6); the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0048] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0049] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 2.
[0050] Example 3
[0051] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0052] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0053] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it three times with deionized water;
[0054] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0055] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0056] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0057] 6) Prepare 300g of 30% hydrogen fluoride solution, add 10g of the sample obtained in step 5), treat with ultrasound at 50°C for 30min, take out the obtained sample, centrifuge and wash it five times, collect the sample, put it in an oven at 100°C for 24h, and the obtained sample is the nano molecular sieve seed crystal, and the particle size of the nano molecular sieve seed crystal is 40% of the particle size before treatment;
[0058] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then adding the nano molecular sieve seed crystals obtained in step 6) in an amount of 10%; stirring continuously for 24 hours to obtain a homogeneous mixture;
[0059] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 150° C. for 48 hours;
[0060] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 3.
[0061] Example 4
[0062] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0063] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0064] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it twice with deionized water;
[0065] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0066] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0067] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0068] 6) preparing 300 g of 30% ammonium fluoride solution, adding 10 g of the sample obtained in step 5), treating with ultrasound at 50° C. for 30 min, taking out the obtained sample, washing it three times by centrifugation, collecting the sample, and drying it in an oven at 100° C. for 24 h. The obtained sample is a nano-molecular sieve seed crystal, and the particle size of the nano-molecular sieve seed crystal is 40% of the particle size before treatment;
[0069] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:15.0; then adding the nano molecular sieve seed obtained in step 6); the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0070] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 150° C. for 48 hours;
[0071] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 4.
[0072] Example 5
[0073] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0074] 1) 80 g of ammonium nitrate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0075] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it three times with deionized water;
[0076] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0077] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0078] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0079] 6) Prepare 300g of 30% ammonium bifluoride solution, add 10g of the sample obtained in step 5), treat with ultrasound at 50°C for 30min, take out the obtained sample, wash it three times by centrifugation, collect the sample, put it in an oven at 100°C for 24h, and the obtained sample is the nano molecular sieve seed crystal, and the particle size of the nano molecular sieve seed crystal is 40% of the particle size before treatment;
[0080] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then adding the nano molecular sieve seed crystals obtained in step 6) in an amount of 10%; stirring continuously for 24 hours to obtain a homogeneous mixture;
[0081] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 130° C. for 48 hours;
[0082] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 5.
[0083] Example 6
[0084] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0085] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0086] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it two to three times with deionized water;
[0087] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0088] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0089] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0090] 6) preparing 300 g of 30% ammonium fluoride solution, adding 10 g of the sample obtained in step 5), treating with ultrasound at 50° C. for 30 min, taking out the obtained sample, washing it by centrifugation for three to five times, collecting the sample, and drying it in an oven at 100° C. for 24 h. The obtained sample is a nano-molecular sieve seed crystal, and the particle size of the nano-molecular sieve seed crystal is 40% of the particle size before treatment;
[0091] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:15.0; then adding the nano molecular sieve seed obtained in step 6); the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0092] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 130° C. for 48 hours;
[0093] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 6.
[0094] Example 7
[0095] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0096] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0097] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it two to three times with deionized water;
[0098] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0099] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0100] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0101] 6) preparing 300 g of 30% ammonium fluoride solution, adding 10 g of the sample obtained in step 5), treating with ultrasound at 50° C. for 30 min, taking out the obtained sample, washing it by centrifugation for three to five times, collecting the sample, and drying it in an oven at 100° C. for 24 h. The obtained sample is a nano-molecular sieve seed crystal, and the particle size of the nano-molecular sieve seed crystal is 40% of the particle size before treatment;
[0102] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then adding the nano molecular sieve seed crystals obtained in step 6) in an amount of 10%; stirring continuously for 24 hours to obtain a homogeneous mixture;
[0103] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 120° C. for 48 h;
[0104] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 7.
[0105] Example 8
[0106] A method for synthesizing a nanomolecular sieve comprises the following steps:
[0107] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0108] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it two to three times with deionized water;
[0109] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0110] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0111] 5) taking out the sample obtained in step 4), filtering and separating it, washing it thoroughly with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 h;
[0112] 6) preparing 300 g of 30% ammonium fluoride solution, adding 10 g of the sample obtained in step 5), treating with ultrasound at 50° C. for 30 min, taking out the obtained sample, washing it by centrifugation for three to five times, collecting the sample, and drying it in an oven at 100° C. for 24 h. The obtained sample is a nano-molecular sieve seed crystal, and the particle size of the nano-molecular sieve seed crystal is 40% of the particle size before treatment;
[0113] 7) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:15.0; then adding the nano molecular sieve seed obtained in step 6); the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0114] 8) placing the mixture obtained in step 7) in a crystallization reactor and crystallizing at 120° C. for 48 h;
[0115] 9) The sample obtained in step 8) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named Example 8.
[0116] Comparative Example 1
[0117] A method for preparing a molecular sieve comprises the following steps:
[0118] 1) adding alkali, aluminum source and silicon source into deionized water in sequence, stirring continuously for 24 hours to obtain a homogeneous mixture; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0;
[0119] 2) placing the mixture obtained in step 1) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0120] 3) The sample obtained in step 2) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named MOR-1;
[0121] Comparative Example 2
[0122] A method for preparing a molecular sieve comprises the following steps:
[0123] 1) adding alkali, aluminum source and silicon source into deionized water in sequence, stirring continuously for 24 hours to obtain a homogeneous mixture; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:15.0;
[0124] 2) placing the mixture obtained in step 1) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0125] 3) The sample obtained in step 2) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named MOR-2.
[0126] Comparative Example 3
[0127] A method for preparing a molecular sieve comprises the following steps:
[0128] 1) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then adding MOR molecular sieve that has not been treated with fluoride as a seed; the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0129] 2) placing the mixture obtained in step 1) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0130] 3) The sample obtained in step 2) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named MOR-3;
[0131] Comparative Example 4
[0132] A method for preparing a molecular sieve comprises the following steps:
[0133] 1) Alkali, aluminum source and silicon source are added to deionized water in sequence, stirred and mixed evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then molecular sieves treated by mechanical crushing (seed particle size is 80% of the particle size before treatment) are added as seeds; the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0134] 2) placing the mixture obtained in step 1) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0135] 3) The sample obtained in step 2) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve, named MOR-4.
[0136] Comparative Example 5
[0137] A method for preparing a molecular sieve comprises the following steps:
[0138] 1) 80 g of ammonium sulfate was dissolved in 800 g of deionized water to obtain a uniform solution, 80 g of existing MOR molecular sieve was added, and the resulting mixture was placed in a magnetic stirrer oil bath at 90° C. and 480 r. for 3 h;
[0139] 2) taking out the sample obtained in step 1), filtering and separating it, and washing it two to three times with deionized water;
[0140] 3) Repeat steps 1) and 2) three times, collect the samples and dry them in an oven at 100°C for 24 hours;
[0141] 4) 63 g of oxalic acid dihydrate was dissolved in deionized water to obtain 750 g of oxalic acid solution, 36 g of the sample obtained in step 3) was added, and the mixture was treated in an oil bath at 90° C. and 650 rpm in a magnetic stirrer for 46 h;
[0142] 5) taking out the sample obtained in step 4), filtering and separating it, washing it with deionized water until it is neutral, collecting the sample and drying it in an oven at 100° C. for 24 hours, and using the obtained sample as a seed crystal, the seed crystal particle size is 60% of the particle size before treatment;
[0143] 6) adding alkali, aluminum source and silicon source to deionized water in sequence, stirring and mixing evenly to obtain a uniform gel; the composition of the gel is SiO2:Al2O3:Na2O:H2O=1:0.079:0.23:38.0; then adding the seed crystals obtained in step 5); the addition amount is 10%; stirring is continued for 24 hours to obtain a homogeneous mixture;
[0144] 7) placing the mixture obtained in step 6) in a crystallization reactor and crystallizing at 170° C. for 48 hours;
[0145] 8) The sample obtained in step 7) was taken out from the crystallization kettle, filtered and separated, washed with deionized water until neutral, and dried in an oven at 100° C. for 24 h to obtain a MOR molecular sieve named MOR-5.
[0146] By comparing the examples with the comparative examples, it can be concluded that the morphological differences of each system are attributed to the different crystallization paths. The specific surface area, pore volume and other data of the prepared samples are shown in Table 1. The specific surface area and mesopore volume of the example samples are significantly higher than those of the comparative example samples, but the micropore volume is basically the same. Observe the scanning electron microscope images of comparative example 1 and comparative example 2 ( Fig.11) It can be seen that the molecular sieve prepared by ordinary hydrothermal synthesis has a dense surface and a large size. When adding seed crystals to the synthesis system, the seed crystals first dissolve into structural units, increase the number of crystal nuclei per unit volume, make the nucleation rate greater than the growth rate of the crystals, and then the gel gradually crystallizes into crystals, which is conducive to the formation of small crystal nuclei. In addition, the addition of seed crystals greatly shortens the crystallization induction period and accelerates the growth rate of the crystals. Subsequently, a high-pressure fixed-bed continuous reaction device was used to evaluate the catalytic performance of the catalyst for DME carbonylation reaction. The results are as follows: Fig.10 As shown, under the same reaction conditions, the embodiment shows the best DME conversion rate, and has the best stability and the longest service life. In summary, the molecular sieve prepared by the method described in the present invention has a smaller crystal size, a more irregular and higher active surface, and is rich in surface hydroxyl groups and irregular mesopores, which is more conducive to promoting crystal growth and can improve mass transfer and diffusion capabilities to a greater extent. The smaller the molecular sieve grains, the shorter the pores, the smaller the intracrystalline diffusion resistance, the stronger the anti-coking ability, and the longer the service life.
[0147] Table 1
[0148]
[0149] Among them, S BET a Specific surface area calculated by BET; S mic b Micropore specific surface area; V mic b Micropore volume, calculated by t-plot; V meso c Mesopore volume = total pore volume - micropore volume.
[0150] The above embodiments are only preferred implementations of the present invention, and are only exemplary descriptions of the technical solutions of the present invention, and are not intended to limit the technical solutions of the present application. For those skilled in the art, several conventional substitutions and improvements can be made without departing from the principles of the present invention, and these conventional substitutions and improvements should also be considered as the protection scope of the present invention.
Claims
1. A method for synthesizing nanomolecular sieves, The following steps are involved: 1) using a fluoride solution to treat the molecular sieve to be used as a seed crystal so that the molecular sieve particles are evenly dispersed; 2) Then, the fluorine-treated molecular sieve is used as a seed crystal, and the molecular sieve is synthesized by a seed crystal-assisted method to obtain a nano molecular sieve product; The method does not use an organic compound structure directing agent and / or a template agent; The fluorine treatment in step 1) is carried out in a fluorine-containing solution, wherein the mass percentage concentration of the fluoride is 5-45wt%; the mass ratio of the molecular sieve to be treated to the fluorine-containing solution is 1:1-1:30, the fluorine treatment temperature is 0°C-100°C, and the treatment time is 10min-24h; the fluoride is one of hydrogen fluoride, ammonium fluoride, and ammonium bifluoride; The crystal size of the molecular sieve after fluorine treatment is reduced to 20-50% of the original size; The molecular sieves described in step 1) and step 2) are molecular sieves with one-dimensional or two-dimensional pore structures or molecular sieves with three-dimensional mesopores and micropores.
2. The method according to claim 1, Features The mass percentage concentration of the fluoride in step 1) is 20-40wt%.
3. The method according to claim 1, Features The treatment process is enhanced by external field, which is ultrasonic treatment.
4. The method according to claim 1, Features The crystal size of the molecular sieve after fluorine treatment is reduced to 30-45% of the original size.
5. The method according to claim 1, Features Before the fluorine treatment in step 1), the molecular sieve is subjected to a pretreatment, wherein the pretreatment is ammonium exchange and acid treatment.
6. The method according to claim 1, Features After the fluorine treatment in step 1), filtering and washing are performed to first obtain a molecular sieve solid, which is then used as a seed to synthesize the molecular sieve.
7. The method according to claim 1, Features The molecular sieve described in step 1) and step 2) is one of MOR, TON and FER.
8. The method according to claim 1, Features The molecular sieve described in step 1) and step 2) is one of MFI and MEL.