A method for preparing bio-based acrylic acid

CN116217378BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310007256.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2024-12-03
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

Existing methods for producing bio-based acrylic acid from lactic acid face challenges such as low conversion rates, poor selectivity, catalyst instability, and high occurrence of side reactions like decarboxylation and decarbonylation, leading to reduced yield and catalyst deactivation.

Method used

A method using an organic metal sulfur halide ion liquid catalyst for the dehydration of lactate to produce bio-based acrylic acid, which includes adding the catalyst and an inhibitor to a lactate aqueous solution for a homogeneous reaction, followed by product separation and optional catalyst recycling, utilizing catalysts like halogenated triethylenediamine metal halide ionic liquids with specific metal ions and structures.

Benefits of technology

The method achieves high single-pass conversion rates of over 95% and selectivity of over 90% for acrylic acid, reduces side reactions, and provides a catalyst with stable performance and long life, facilitating easy separation and recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004036085750000041
    Figure BDA0004036085750000041
  • Figure BDA0004036085750000051
    Figure BDA0004036085750000051
  • Figure BDA0004036085750000081
    Figure BDA0004036085750000081
Patent Text Reader

Abstract

The invention relates to a method for preparing bio-based acrylic acid. The method comprises the steps of preparing acrylic acid, acrylic acid salt or a mixture thereof by homogeneous dehydration reaction with a lactate aqueous solution as a raw material under the catalytic action of an organic metal sulfur halide ion liquid, obtaining acrylic acid after acidification and separation of the reaction product, and recycling the catalyst. The method of the invention has high yield and selectivity of the target product, and has stable process, simple operation, low energy consumption, and the catalyst can be recycled, thus solving the problems of poor selectivity of the lactic acid (ester / salt) dehydration process reaction, unstable catalyst, rapid deactivation and difficult regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic chemical synthesis, and particularly relates to a method for preparing bio-based acrylic acid. Background Art

[0002] Acrylic acid is an extremely important bulk chemical, mainly used as a polymer monomer and organic chemical raw material. Its derivatives are widely used in coatings, adhesives, leather, textiles, plastic processing, packaging materials, personal care and other fields.

[0003] At present, acrylic acid in industry is mainly produced by a two-step oxidation process with petrochemical-based propylene as raw material, and the yield of acrylic acid in the whole process is about 87-88%. The production of acrylic acid from petroleum derivatives increases greenhouse gas emissions. With the increasing shortage of oil resources, the demand for carbon emission reduction is becoming more and more urgent. The voice and demand for bio-based materials and chemicals are getting higher and higher, especially in the fields of personal care, polyester, food, etc. The EU, the United States and China are all seeking to develop key bio-based materials to replace petrochemical-based products, and have set corresponding goals. The world's four largest acrylic acid producers, BASF, Dow Chemical, Arkema and Nippon Catalyst, are all developing and researching bio-based acrylic acid production processes. The synthesis methods of bio-based acrylic acid mainly include lactic acid, 3-hydroxypropionic acid dehydration method and glycerol dehydration oxidation method. Among them, lactic acid is one of the main products of biomass fermentation. This technology has achieved large-scale industrial lactic acid production with high yield and low cost, and it is possible to ferment it with cheaper plant cellulose as raw material in the future. Using lactic acid as raw material, the production of bio-based acrylic acid through lactic acid dehydration process is expected to achieve industrial production in the future.

[0004] The main catalytic systems for dehydration of lactic acid (salt / ester) mainly include metal salt catalytic systems, modified molecular sieve catalyst systems, supported acidic catalytic systems, metal oxides and alkaline substances. Patent US2859240 uses alkali metals, alkaline earth metals and rare earth metal salts as catalysts, among which sodium phosphate and calcium sulfate have the best performance, and the acrylic acid yield reaches 68%; Patent US4786756 uses phosphoaluminic acid as a catalyst and ammonium lactate as a raw material, with a reaction conversion rate of 100% and an acrylic acid selectivity of 61.1%; a higher acrylic acid selectivity can be obtained on salt catalysts, but the catalyst has a small specific surface area and few active sites, which on the one hand causes a low conversion rate of lactic acid or lactate esters, and on the other hand causes poor catalyst stability and difficulty in regeneration. Patent CN101352688A discloses that a 100% lactic acid conversion rate and 63% acrylic acid selectivity can be obtained by using one of inorganic porous materials such as silicon aluminum molecular sieve, phosphorus aluminum molecular sieve and mesoporous material as a carrier and one or more of active metals such as Li, Na, K, Ca, Mg, Ba, etc. as active components; CN101049571B discloses a HZSM-5 / NaY catalyst modified with composite molecular sieve potassium, with a lactic acid conversion rate of 99% and an acrylic acid selectivity of more than 70%; Patent CN101602010B discloses a 100% lactic acid conversion rate and 63% acrylic acid selectivity by using aqueous alkali (such as NH3, NaOH and Na 2CO3) or phosphate (such as NaH2PO4, LiH2PO4, LaPO4, etc.) modified ZSM-5 molecular sieve as a catalyst, the best yield of acrylic acid obtained from lactic acid dehydration is 83.9%; Patent CN102019193A uses a composite of molecular sieve and montmorillonite as a catalyst, the lactic acid dehydration conversion rate can reach 95%, and the acrylic acid selectivity can reach more than 90%; although the regeneration process of molecular sieve catalysts is mature, their strong acid sites are not conducive to the formation of acrylic acid, and it is difficult to change the molecular sieve structure by modification to completely eliminate the strong acid sites, which intensifies the side reactions and limits the yield of the target product. Patent US4729978 uses NaH2PO4 / SiO2 as a catalyst, and the acrylic acid yield is 58%; Patent CN102029176A uses a supported molecular sieve Na2HPO4 / NaY as a catalyst, and the lactic acid conversion rate can reach 85.3%, and the acrylic acid selectivity can reach 68.5%; Patent CN102091647B uses a supported molecular sieve Na2HPO4 / small particle size NaY as a catalyst, and the acrylic acid yield can reach 74.3%; The loading method has limited control over the acidity and alkalinity of the catalyst surface, and the loading may cover the medium and strong acid active sites that are beneficial to the formation of acrylic acid, thereby reducing the reaction efficiency.

[0005] Decarboxylation and decarbonylation are very likely to occur during the dehydration of lactic acid (ester), resulting in a significant increase in byproducts such as acetaldehyde, 2,3-pentanedione, propionic acid, CO, and CO2, while reducing the service life of the catalyst and affecting the terminal application of acrylic acid products. Using lactate as a raw material to protect the carboxyl group can significantly reduce the occurrence of side reactions. Lactate is a raw material for producing lactic acid. Directly using lactate as a raw material can reduce lactate acidification and post-treatment steps, thereby reducing raw material costs.

[0006] Therefore, finding a catalyst with high catalytic efficiency, good target product selectivity, strong stability and long catalytic life has always been the focus of research on the process of dehydrating lactic acid (salt / ester) to prepare bio-based acrylic acid. Summary of the invention

[0007] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a catalyst for preparing bio-based acrylic acid by dehydration of lactate and a corresponding reaction process, wherein the catalyst has high catalytic efficiency, good target product selectivity, strong stability, and long catalytic life. In order to achieve the above-mentioned invention purpose and the above-mentioned technical effect, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing bio-based acrylic acid, the method comprising the following steps:

[0009] S1: adding a catalyst and an inhibitor to a lactate aqueous solution to prepare acrylic acid and acrylic acid salt by homogeneous reaction;

[0010] S2: The product is acidified and separated to obtain acrylic acid;

[0011] Optionally, S3: the catalyst is recycled.

[0012] Wherein, the catalyst described in S1 is an organic metal sulfur halide ion liquid catalyst.

[0013] In the present invention, the organic metal halide ionic liquid catalyst described in S1 is one or more of halogenated triethylenediamine metal halide ionic liquid, halogenated quaternary ammonium salt metal halide ionic liquid, and halogenated pyrrolidone metal halide ionic liquid, and their structures are shown below:

[0014]

[0015] wherein Y and Z in the cation are respectively one of H, COOH, HSO3, H2PO4, R1, R2, R3, R4 are respectively one of C1-C6 alkanes, preferably one of C1-C2 alkanes; m is an integer of 0-5, preferably an integer of 1-3; x is selected from 1-3; a is selected from an integer of 0-4, preferably an integer of 1-3; the metal ions in M(SCl6)x are respectively Cu + 、Zn 2+Mg 2+ Sn 2+ 、Ni 2+ 、Al 3+ , Fe 3+ 、Mo 3+ 、Bi 3+ , Ir 3+ Cr 3+ 、Au 3+ 、Zr 4+ 、Ce 4+ 、In 4+ One or more of, preferably Cu + Sn 2+ 、Al 3+ , Ir 3+ Cr 3 + 、Ce 4+ One or more of; preferably, based on the total weight of the lactate aqueous solution, the addition amount of the organic metal halide ion liquid catalyst is 0.5wt.%-10wt.%, preferably 1wt.%-5wt.%.

[0016] In a specific embodiment, the organometallic halide ionic liquid is selected from at least one of the following structural formulas A, B, C, D, E, F, G, and H:

[0017]

[0018] The dehydration reaction of lactate to produce bio-based acrylic acid can greatly reduce the occurrence of side reactions such as decarboxylation and decarbonylation by protecting the carboxyl functional group, but the key to the reaction is to find a catalyst with high catalytic efficiency, good target product selectivity, strong stability, and long catalytic life. The applicant experimentally found that organic metal halide ionic liquid can be used as a catalyst for the dehydration of lactate to produce bio-based acrylic acid. The catalyst has excellent catalytic activity and solubility, combining the dual advantages of catalyst and solvent, and has Lewis acid / Bronsted acid active sites with moderate acid strength and easy to control, and can overcome the mass transfer resistance in the dehydration process of lactate, thereby improving the reaction efficiency; the reaction process is mild, which solves the problem of lactate decomposition, and the extremely low volatility and structural adjustability of the ionic liquid simplify the recovery operation.

[0019] In the method of the present invention, the organic metal halide ionic liquid catalyst can be synthesized by any method known to those skilled in the art for synthesizing ionic liquids with similar structures, or can be prepared by referring to the preparation method in the following literature, such as "Bronsted-Lewis diacidic ionic liquid catalytic synthesis of lactide" (Chemical Industry and Engineering, 2017). In some specific embodiments of the present invention, the specific preparation process is as follows:

[0020] A certain amount of ionic liquid precursor is taken into a three-necked flask, and a metal halide is added to the ionic liquid according to a molar ratio of halide to ionic liquid precursor of 1:2-2:1, and the reaction is carried out under a nitrogen atmosphere at 80-140°C for 6-24 hours to obtain organic metal halide ionic liquids with different structures and ratios; the metal halide is dissolved in a solvent of dichloromethane at a volume ratio of 1:1-1:15, and sulfur is added to the metal halide solution at a molar ratio of 1:5-5:1, and the reaction is carried out for 12-24 hours, and then the organic metal sulfur halide ionic liquid is obtained by cooling at -30°C to -50°C.

[0021] In the present invention, the lactate in S1 is selected from one or more of lithium lactate, sodium lactate, potassium lactate, calcium lactate, barium lactate, strontium lactate, and cesium lactate; preferably, the mass concentration of the lactate aqueous solution is 10wt.% to 70wt.%, preferably 15wt.% to 40wt.%.

[0022] In the present invention, the inhibitor described in S1 is selected from one or more of phenolic inhibitors, quinone inhibitors, and nitrogen free radical inhibitors, preferably one or more of hydroquinone, tert-butylhydroquinone, p-benzoquinone, methylhydroquinone, ZJ-701, ZJ-702, and ZJ-705, and more preferably one or more of hydroquinone, ZJ-701, and ZJ-705; preferably, based on the total weight of the lactate aqueous solution, the addition amount of the inhibitor is 0.1wt.%-5wt.%, preferably 0.25wt.%-2wt.%.

[0023] In the present invention, the homogeneous reaction described in S1 is carried out in a tank reactor; preferably, the reaction pressure is 1-10 MPaG, preferably 2-4 MPaG, the reaction temperature is 180°C-250°C, preferably 200-240°C, and the reaction time is 0.5-5h, preferably 1-3h.

[0024] In the present invention, after the reaction product in S2 is acidified, it is distilled in a lightness removal tower to remove light components, distilled and dehydrated in a dehydration tower, and distilled in an acrylic acid refining tower to remove heavy components, and an acrylic acid product is obtained at the top of the tower; preferably, the acidification adopts a dilute sulfuric acid solution with a concentration of 5-20wt%; preferably, the pressure of the lightness removal tower is 70-100kPaA, and the tower bottom temperature is 50-75°C; preferably, the pressure of the dehydration tower for distillation and dehydration is 20-60kPaA, and the tower bottom temperature is 80-106°C; preferably, the pressure of the acrylic acid refining tower is 1-10kPaA, and the tower top temperature is 80-120°C.

[0025] In the present invention, the catalyst described in S3 is continuously recycled after being washed with a solvent and dried in vacuo; preferably, the washing solvent is one or more of alcohols, esters, ethers, ketones, and chlorinated alkanes, preferably one or more of methanol, ethanol, and ether.

[0026] Another object of the present invention is to provide a bio-based acrylic acid.

[0027] A bio-based acrylic acid is prepared by using the above preparation method.

[0028] Compared with the prior art, the present invention has the following positive effects:

[0029] (1) The lactate dehydration method of the present invention can achieve a single-pass conversion rate of greater than 95%, an acrylic acid (salt) selectivity of greater than 90%, effectively inhibits the occurrence of side reactions such as decarbonylation and decarboxylation, has high reaction efficiency, and good selectivity for the target product.

[0030] (2) The catalyst has the dual advantages of an acidic catalyst and a solvent. The acid strength and surface acid sites are adjustable, and the reaction mass transfer resistance is small.

[0031] (3) The catalyst is easy to prepare, has stable performance, long catalytic life, and is easy to separate and recycle, solving the problem of instability and easy deactivation of traditional catalysts.

[0032] (4) The method of the present invention is easy to operate, has a mild process, a simple flow, low energy consumption, and obvious cost advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 For Preparation Example 1 1 H NMR (600 MHz, 298 K) characterization results;

[0034] Figure 2 For the preparation of Example 5 1 H NMR (600 MHz, 298 K) characterization results;

[0035] Figure 3 For the preparation of Example 8 1 H NMR (600 MHz, 298 K) characterization results. DETAILED DESCRIPTION

[0036] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0037] The main sources of raw materials are as follows:

[0038] Table 1 Main reaction materials

[0039]

[0040]

[0041] Preparation Example: Preparation of organic metal halide ion liquid catalysts A to H:

[0042]

[0043] Catalyst Characterization: 1 H NMR: The ionic liquid was dissolved in an organic solvent (CDCl3) and characterized by hydrogen spectrum using a nuclear magnetic resonance spectrometer (JNM-ECA 600 MHz, Bruker, Switzerland).

[0044] Preparation Example 1: Preparation of Catalyst A

[0045] Take 20 mmol of ionic liquid precursor trimethylammonium chloride in a three-necked flask, add SnCl2 to the ionic liquid at a molar ratio of halide to ionic liquid precursor of 0.67, react under a nitrogen atmosphere, react at 120°C for 12 hours to obtain an organic metal halide ionic liquid, dissolve the ionic liquid in CH2Cl2 at a volume ratio of 1:5, add S to the ionic liquid solution at a molar ratio of 1.2:1, react at room temperature for 16 hours, and slowly cool to -40°C to obtain catalyst A.

[0046] Preparation Example 2: Preparation of Catalyst B

[0047] Take 18 mmol of ionic liquid precursor trihexylpentanesulfonic acid ammonium chloride in a three-necked flask, add AlCl3 to the ionic liquid at a molar ratio of aluminum chloride to ionic liquid precursor of 0.8, react under a nitrogen atmosphere, react at 110°C for 12 hours to obtain an organic metal halide ionic liquid, dissolve the ionic liquid in CH2Cl2 at a volume ratio of 1:10, add sulfur to the ionic liquid solution at a molar ratio of 2:1, react at room temperature for 20 hours, and slowly cool to -30°C to obtain catalyst B.

[0048] Preparation Example 3: Preparation of Catalyst C

[0049] Take 25 mmol of ionic liquid precursor tributyl methyl ammonium chloride in a three-necked flask, add ZnCl2 to the ionic liquid at a molar ratio of zinc chloride to ionic liquid precursor of 1, react under a nitrogen atmosphere, react at 80°C for 24 hours to obtain an organic metal halide ionic liquid, dissolve the ionic liquid in CH2Cl2 at a volume ratio of 1:15, add sulfur to the ionic liquid solution at a molar ratio of 5:1, react at room temperature for 24 hours, and slowly cool to -50°C to obtain catalyst C.

[0050] Preparation Example 4: Preparation of Catalyst D

[0051] 25mmol of triethylenediamine was dissolved in 50ml of ethyl acetate, and then reacted with 52mmol of 1,3-propane sultone at 60°C for 24h, and acidified with hydrochloric acid at a molar ratio of 1:1 to sultone to obtain triethylenediamine chloropropanesulfonic acid ionic liquid; 20mmol of ionic liquid precursor triethylenediamine chlorosulfonic acid ionic liquid was taken in a three-necked flask, CeCl4 was added to the ionic liquid at a molar ratio of cerium chloride to ionic liquid precursor of 2, and the reaction was carried out under a nitrogen atmosphere at 90°C for 10h to obtain an organic metal halide ionic liquid, and the ionic liquid was dissolved in CH2Cl2 at a volume ratio of 1:10, and sulfur was added to the ionic liquid solution at a molar ratio of 2.2:1, and the reaction was carried out at room temperature for 18h, and the catalyst D was slowly cooled to -40°C.

[0052] Preparation Example 5: Preparation of Catalyst E

[0053] 15mmol triethylenediamine and 32mmol chloropropylsulfonic acid were reacted at 50°C for 4h to obtain an ionic liquid precursor triethylenediamine chloropropionic acid ionic liquid. 10mmol of the ionic liquid precursor was taken into a three-necked flask, and IrCl3 was added to the ionic liquid at a molar ratio of iridium chloride to ionic liquid precursor of 0.5. The reaction was carried out under a nitrogen atmosphere and reacted at 90°C for 12h to obtain an organic metal halide ionic liquid. The ionic liquid was dissolved in CH2Cl2 at a volume ratio of 1:1, and sulfur was added to the ionic liquid solution at a molar ratio of 2:1. The reaction was carried out at room temperature for 12h and the catalyst E was obtained.

[0054] Preparation Example 6: Preparation of Catalyst F

[0055] 20mmol of triethylenediamine and 40mmol of chloroethylphosphoric acid were reacted at 60°C for 5h to obtain an ionic liquid precursor triethylenediamine chloroethylphosphoric acid ionic liquid. 15mmol of the ionic liquid precursor was placed in a three-necked flask, AlCl3 was added to the ionic liquid at a molar ratio of aluminum chloride to the ionic liquid precursor of 1, and the reaction was carried out under a nitrogen atmosphere at 140°C for 6h to obtain an organic metal halide ionic liquid. The ionic liquid was dissolved in CH2Cl2 at a volume ratio of 1:10, and sulfur was added to the ionic liquid solution at a molar ratio of 1.5:1. The reaction was carried out at room temperature for 16h, and the catalyst F was obtained.

[0056] Preparation Example 7: Preparation of Catalyst G

[0057] 24mmol of methyl pyrrolidone and hydrochloric acid are acidified at room temperature in an equimolar ratio to obtain a precursor methyl pyrrolidone chloride; 20mmol of the precursor methyl pyrrolidone chloride is taken in a three-necked flask, InBr4 is added to the ionic liquid in a molar ratio of indium chloride to ionic liquid precursor of 0.5, and the reaction is carried out under a nitrogen atmosphere at 100°C for 24h to obtain an organic metal halide ionic liquid, and the ionic liquid is dissolved in CH2Cl2 at a volume ratio of 1:10, and sulfur is added to the ionic liquid solution at a molar ratio of 4:1, and the reaction is carried out at room temperature for 24h, and slowly cooled to -40°C to obtain a catalyst G.

[0058] Preparation Example 8: Preparation of Catalyst H

[0059] 25mmol of ethyl pyrrolidone and hydrochloric acid were acidified at room temperature in an equimolar ratio to obtain a precursor of ethyl pyrrolidone chloride; 20mmol of ionic liquid precursor ethyl pyrrolidone chloride was taken in a three-necked flask, AlCl3 was added to the ionic liquid in a molar ratio of aluminum chloride to ionic liquid precursor of 0.5, and the reaction was carried out under a nitrogen atmosphere at 80°C for 24h to obtain an organic metal halide ionic liquid, and the ionic liquid was dissolved in CH2Cl2 at a volume ratio of 1:10, and sulfur was added to the ionic liquid solution at a molar ratio of 1:5, and the reaction was carried out at room temperature for 24h, and the catalyst H was obtained.

[0060] Examples 1-9

[0061] In a 1.9L reactor, 1kg of lactate aqueous solution was added in a certain proportion, and a polymerization inhibitor, hydroquinone, and an organic metal halide ion liquid catalyst were added in a certain proportion, and the reaction was stirred for a certain time at a certain temperature and pressure to obtain the target product, acrylic acid / acrylic acid salt, and the conversion rate and selectivity were calculated by sampling and analysis. The specific conditions and results of each embodiment are shown in Table 2.

[0062] Comparative Example 1

[0063] The process conditions of Comparative Example 1 are consistent with those of Example 5, except that the catalyst E in Example 5 is replaced by NaH2PO4.

[0064] Comparative Example 2

[0065] The process conditions of Comparative Example 2 are consistent with those of Example 5, except that the catalyst E in Example 5 is replaced by ZSM-5 molecular sieve.

[0066] Table 2 Lactate dehydration process conditions and effects

[0067]

[0068]

[0069] Embodiment 10-11

[0070] Example 10

[0071] Acrylic acid separation and recycling of ionic liquid catalyst: 1 kg of the reaction solution obtained in Example 2 was acidified by adding 5 wt.% of dilute sulfuric acid solution, and the molar ratio of sodium ion to hydrogen ion was 1:1, and the acrylate was completely acidified; the filtrate was distilled at a pressure of 70 kPaA to remove the light components in the reaction solution, and the bottom temperature was 50°C, and then toluene was added to the system as an azeotropic agent at a volume ratio of toluene to water of 1:1, and water was removed by reduced pressure azeotropic distillation, and the bottom temperature was 92°C at a pressure of 50 kPaA, and then the tower was The kettle liquid continued to be refined, with a pressure of 6 kpaA and a kettle temperature of 110°C. An acrylic acid product with a purity greater than 99% was obtained at the top of the tower. The catalyst in the kettle was washed with ethanol three times and the sodium salt was filtered out; it was then washed with ether three times, placed in a drying oven at 90°C and a high vacuum of 10Pa for 24 hours and then recycled. After the catalyst was used five times, there was no obvious attenuation in activity, the reaction conversion rate could reach 96.1%, the selectivity of acrylic acid and acrylic acid salt was 92.5%, the single-recycle acrylic acid yield was higher than 85%, and no new impurities were found in the reaction system.

[0072] Embodiment 11

[0073] To 1 kg of the reaction solution obtained in Example 5, a 10% dilute sulfuric acid solution was added dropwise for acidification. According to the molar ratio of calcium ions to sulfate ions of 1:1, a precipitate was continuously precipitated in the solution. When no calcium salt continued to precipitate in the solution, the addition of sulfuric acid solution was stopped, and the filtrate was obtained by filtration. The filtrate was distilled at a pressure of 80 kPaA to remove the light components in the reaction solution. The bottom temperature was 62°C. Then, toluene was added to the system as an azeotropic agent at a volume ratio of toluene to water of 1:1. Water was removed by reduced pressure azeotropic distillation. At a pressure of 40 kPaA, the bottom temperature was 42°C. The temperature is about 85°C, and then the bottom liquid is further refined with a pressure of 4 kpaA and a bottom temperature of 105°C. An acrylic acid product with a purity greater than 99% is obtained at the top of the tower. The bottom catalyst is washed 3 times with ether and ethyl acetate respectively, placed in a drying oven at 80°C and high vacuum 5Pa for 24 hours and then recycled. After the catalyst has been used 8 times, there is no obvious attenuation in activity, the reaction conversion rate can reach 95.5%, the selectivity of acrylic acid and acrylic acid salt is 92.2%, the single-recycle acrylic acid yield is higher than 85%, and no new impurities are found in the reaction system.

[0074] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A method for preparing bio-based acrylic acid, characterized in that: The method comprises the following steps: S1: adding a catalyst and an inhibitor to a lactate aqueous solution to prepare acrylic acid and acrylic acid salt by homogeneous reaction; S2: The product is acidified and separated to obtain acrylic acid; Optionally, S3: the catalyst is recycled. Wherein, the catalyst described in S1 is an organic metal sulfur halide ion liquid catalyst.

2. The preparation method according to claim 1, characterized in that: The organic metal halide ionic liquid catalyst described in S1 is one or more of halogenated triethylenediamine metal halide ionic liquid, halogenated quaternary ammonium salt metal halide ionic liquid, and halogenated pyrrolidone metal halide ionic liquid, and their structures are shown below: Wherein, Y and Z in the cation are respectively one of H, COOH, HSO3, H2PO4, R1, R2, R3, R4 are respectively one of C1-C6 alkanes; m is an integer of 0-5; x is selected from 1-3; a is selected from an integer of 0-4; the metal ions in M(SCl6)x are respectively Cu + 、Zn 2+ Mg 2+ Sn 2+ 、Ni 2+ 、Al 3+ , Fe 3+ 、Mo 3+ 、Bi 3+ , Ir 3+ Cr 3+ 、Au 3+ 、Zr 4+ 、Ce 4+ 、In 4+ One or more of .

3. The preparation method according to claim 2, characterized in that: In the organic metal halide ionic liquid catalyst described in S1, R1, R2, R3, and R4 are respectively one of C1-C2 alkanes; m is an integer of 1-3; a is an integer selected from 1-3; the metal ions in M(SCl6)x are respectively Cu + Sn 2+ 、Al 3+ , Ir 3+ Cr 3+ 、Ce 4+ One or more of; Based on the total weight of the lactate aqueous solution, the added amount of the organic metal halide ion liquid catalyst is 0.5wt.%-10wt.%.

4. The preparation method according to claim 3, characterized in that: In S1, the addition amount of the organic metal halide ion liquid catalyst is 1 wt.%-5 wt.% based on the total weight of the lactate aqueous solution.

5. The preparation method according to claim 1 or 2, characterized in that: S1 The lactate is selected from one or more of lithium lactate, sodium lactate, potassium lactate, calcium lactate, barium lactate, strontium lactate and cesium lactate.

6. The preparation method according to claim 5, characterized in that: The mass concentration of the aqueous solution of lactate in S1 is 10wt.% to 70wt.%.

7. The preparation method according to claim 6, characterized in that: The mass concentration of the aqueous solution of lactate in S1 is 15wt.%-40wt.%.

8. The preparation method according to claim 1, characterized in that: S1 The inhibitor is selected from one or more of phenolic inhibitors, quinone inhibitors, and nitrogen free radical inhibitors.

9. The preparation method according to claim 8, characterized in that: S1 The inhibitor is one or more of hydroquinone, tert-butyl hydroquinone, p-benzoquinone, methyl hydroquinone, ZJ-701, ZJ-702, and ZJ-705; Based on the total weight of the lactate aqueous solution, the addition amount of the polymerization inhibitor is 0.1wt.%-5wt.%.

10. The preparation method according to claim 9, characterized in that: S1 The inhibitor is one or more of hydroquinone, ZJ-701, and ZJ-705; Based on the total weight of the lactate aqueous solution, the added amount of the polymerization inhibitor is 0.25wt.%-2wt.%.

11. The preparation method according to claim 1, characterized in that: The homogeneous reaction described in S1 is carried out in a tank reactor.

12. The preparation method according to claim 11, characterized in that: The reaction pressure in S1 is 1-10 MPaG, the reaction temperature is 180°C-250°C, and the reaction time is 0.5-5h.

13. The preparation method according to claim 12, characterized in that: The reaction pressure in S1 is 2-4 MPaG, the reaction temperature is 200-240°C, and the reaction time is 1-3h.

14. The preparation method according to claim 1, characterized in that: After the reaction product in S2 is acidified, it is distilled in a light-removing tower to remove light components, distilled in a dehydration tower to dehydrate, and distilled in an acrylic acid refining tower to remove heavy components, and an acrylic acid product is obtained at the top of the tower.

15. The preparation method according to claim 14, characterized in that: In S2, the acidification uses a dilute sulfuric acid solution with a concentration of 5-20wt%; The pressure of the lightness removal tower is 70-100 kPaA, and the temperature of the tower bottom is 50-75°C; The dehydration tower pressure of distillation dehydration is 20-60kPaA, and the tower bottom temperature is 80-106℃; The pressure of the acrylic acid refining tower is 1-10kPaA, and the top temperature is 80-120℃.

16. The preparation method according to claim 1, characterized in that: The catalyst in S3 is washed with solvent and dried in vacuum before being recycled.

17. The preparation method according to claim 16, characterized in that: In S3, the washing solvent is one or more of alcohols, esters, ethers, ketones, and chlorinated alkanes.

18. The preparation method according to claim 17, characterized in that: In S3, the washing solvent is one or more of methanol, ethanol, and ether.