A method for catalytically pyrolyzing polycarbonate plastics to alkylene oxides

By using a metal complex catalyst with a porphyrin or phthalocyanine structure as the skeleton to catalyze the pyrolysis of polycarbonate under solvent-free conditions, the problems of unstable catalyst structure and solvent usage are solved, and efficient and sustainable monomer recovery and cost are achieved. reduce.

CN116217517BActive Publication Date: 2024-10-01DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310248855.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-15
Publication Date
2024-10-01
Estimated Expiration
2043-03-15

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively catalyze the pyrolysis of polycarbonate into alkylene oxide monomers under solvent-free conditions, and the catalyst structure is unstable and cannot be used repeatedly in the polymer recovery process, which limits the industrial application of polycarbonate.

Method used

A metal complex catalyst with a porphyrin or phthalocyanine structure as the skeleton is used, combined with a cocatalyst, to perform catalytic pyrolysis under negative pressure conditions of 100 to 250°C. The molar ratio of the catalyst to polycarbonate is 1:10 to 1: 10000, the reaction time is 0.1 to 24 hours, realizing the direct degradation of polycarbonate into alkylene oxide monomer and carbon dioxide.

Benefits of technology

Efficient and rapid recovery of pure monomers under solvent-free conditions is achieved. The catalyst maintains high activity and selectivity, and can continuously recover target monomers, reducing costs and avoiding the need for polymer waste sorting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116217517B_ABST
    Figure CN116217517B_ABST
Patent Text Reader

Abstract

The invention relates to a method for pyrolysis and recovery of polycarbonate plastics. Polycyclohexene carbonate is the most common structure, which has excellent tensile strength, high glass transition temperature, and excellent oxygen and water barrier properties, and is a green sustainable plastic. Although carbon dioxide is cheap, the preparation cost of another monomer, cyclohexene oxide, is high, which limits its large-scale industrial application. Using metal porphyrin or metal phthalocyanine as a catalyst can achieve the degradation of polycyclohexene carbonate to cyclohexene oxide monomer, wherein the conversion rate and selectivity can reach 99%, and the monomer can also be polymerized with carbon dioxide again through treatment, thereby achieving resource reuse, and providing a practical solution to solve the problem of high monomer cost of polycyclohexene carbonate. This catalyst can catalyze the pyrolysis of most alicyclic polycarbonates to cycloalkylene oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for pyrolysis and recovery of polycarbonate plastics. Polycyclohexene carbonate is the most common structure, which has excellent tensile strength, high glass transition temperature, and excellent oxygen and water barrier properties, and is a green sustainable plastic. Although carbon dioxide is cheap, the preparation cost of another monomer, cyclohexene oxide, is high, which limits its large-scale industrial application. Using metal porphyrin or metal phthalocyanine as a catalyst can achieve the degradation of polycyclohexene carbonate to cyclohexene oxide monomer, wherein the conversion rate and selectivity can reach 99%, and the monomer can also be polymerized with carbon dioxide again through treatment, thereby achieving resource reuse, and providing a practical solution to solve the problem of high monomer cost of polycyclohexene carbonate. This catalyst can catalyze the pyrolysis of most alicyclic polycarbonates to cycloalkylene oxide. Background Art

[0002] Since its birth in the last century, polymer plastics have played an important role in all aspects of human society and promoted the development of human civilization. Due to the chemical inertness of plastics and their short service life, a large amount of plastic waste will be generated, and the continuous accumulation will cause serious environmental pollution problems. Therefore, closed-loop recycling from polymers to monomers has received widespread attention and has become an emerging research field in synthetic polymers. It has been listed as one of the top ten emerging technologies in the field of chemistry by IUPAC for two consecutive years.

[0003] Carbon dioxide-based polycarbonate uses cheap C1 resources as raw materials, has unique biodegradability and biocompatibility, and is a typical representative of environmentally friendly, green and sustainable polymer materials. However, most carbon dioxide-based polycarbonates can only obtain thermodynamically stable cyclic carbonates during pyrolysis, which are difficult to repolymerize back to polymers, and there are very few examples of truly achieving closed-loop recycling to monomers.

[0004] Polycyclohexene carbonate (PCHC) is a widely studied material with excellent tensile strength and excellent oxygen and water barrier properties. In 2022, British Professor Williams (Angew.Chem.Int.Ed.2022,61,e202201785) and Professor Zhang Yuetao (Chem.Sci.2022,13,6283) used different bimetallic zinc catalysts to achieve the chemical recovery of alkylene oxide monomers in toluene solution of PCHC. However, the use of toluene brings about the problem of solvent separation, which increases the cost of recycling. The use of bulk pyrolysis can avoid the use of large amounts of organic solvents and is a method with more industrial prospects. Our research group used commercialized metal Schiff base Cr III-Salen and quaternary ammonium salts are used as catalysts (Angew.Chem.Int.Ed.2022,61,e202204492) to achieve thermal decomposition and recovery of alicyclic carbon dioxide-based polycarbonates of various structures under solvent-free conditions. However, this type of Salen catalyst has the disadvantages of unstable structure and easy decomposition by heat. It cannot be used repeatedly in the process of polymer recovery and has no industrial application prospects. Therefore, we seek a catalyst with more stable structure for the catalytic pyrolysis of polycarbonate. Summary of the invention

[0005] The technical problem to be solved by the present invention is to develop a stable catalyst for catalyzing the thermal decomposition of polycarbonate into alkylene oxide monomers, and the metal porphyrin catalyst is characterized in that the metal porphyrin catalyst has high stability, high activity and simple structure.

[0006] A method for catalytic pyrolysis of polycarbonate plastics, under the reaction temperature of 100 to 250°C and solvent-free negative pressure conditions, using a catalyst to directly degrade the polycarbonate plastic into alkylene oxide monomers and carbon dioxide; the molar ratio of the catalyst to the repeating unit in the polycarbonate in the catalytic pyrolysis reaction system is 1:10 to 1:10000, and the reaction time is 0.1 to 24 hours.

[0007] The catalyst is a metal complex catalyst 1 with a porphyrin structure as a skeleton or a metal complex catalyst 2 with a phthalocyanine structure as a skeleton; the structural formulas of the two are as follows:

[0008]

[0009] in,

[0010] H, Me, Et;

[0011] M=Ga, Cr, Al, Fe;

[0012] M1=Cr, Al, Mg, Zn, Cu.

[0013] Adding co-catalyst R into the reaction system 1 R 2 3YX 1 , where R 1 R 2 3 is the cationic part of the cocatalyst, which is tetramethyl, tetraethyl, tetrabutyl, tetrapropyl, benzyltriethyl, benzyltripropyl, benzyltributyl, hexadecyltrimethyl, dodecyltrimethyl, bis-(triphenylphosphorane), butyltriphenyl, benzyltriphenyl or propyltriphenyl, and Y is nitrogen or phosphorus; X 1 Cl -1 Br -1,I -1 、NO3 -1 、CH3COO -1 、ClO4 -1 、BF4 -1 OH -1 ,BPh4 -1 or N3 -1 Monovalent anion; the molar ratio of the co-catalyst to the catalyst is not greater than 10.

[0014] The polycarbonate plastic is suitable for alicyclic polycarbonate with a molecular weight of 1 to 1000 kg / mol and a molecular weight distribution of 1.0 to 5.0, and the structure is as follows:

[0015]

[0016] Other polymer materials may also exist in the reaction system.

[0017] The polymer materials include double A polycarbonate, polystyrene, polypropylene, high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polyamide, polyethylene terephthalate, polyhydroxyalkanoate, and polylactic acid.

[0018] Beneficial effects of the present invention:

[0019] (1) The porphyrin and phthalocyanine contained in the present invention are two kinds of macromolecular heterocyclic compounds with high conjugation, high stability, simple synthesis and low cost.

[0020] (2) The catalyst of the present invention can be used to quickly recover pure monomers under solvent-free conditions and has high activity.

[0021] (3) The present invention relates to a method for recycling polymers, which can continuously recover target monomers by intermittent feeding, while the catalyst still maintains high activity and selectivity.

[0022] (4) The present invention can selectively depolymerize polycarbonate from a variety of polymer waste materials to recover monomers without the need to sort and classify the polymer waste, thereby reducing costs and saving resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the H-NMR spectrum of polycyclohexene carbonate.

[0024] Figure 2 This is the H-NMR spectrum of cyclohexane oxide, the thermal decomposition product of polycyclohexene carbonate. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.

[0026] Example 1

[0027] A method for catalytic pyrolysis of polycarbonate plastics, comprising the following steps:

[0028] In a reaction bottle, add in the following order at ambient temperature: a certain amount of main catalyst, co-catalyst, and 5 g of polymer; after adding dichloromethane to completely dissolve the catalyst and polymer, remove the solvent under negative pressure and seal the device, quickly raise the temperature to the required temperature, stop the reaction after the specified reaction time, and use Varian INOVA-400MHz to measure the reaction liquid nuclear magnetic resonance to calculate the conversion rate of the polymer in the degradation reaction and the selectivity of the product.

[0029] Table 1 Catalytic pyrolysis reaction of polycyclohexene carbonate

[0030]

[0031]

[0032]

[0033]

[0034]

[0035] Note 1: The molar ratio refers to catalyst:cocatalyst:polymer repeating unit;

[0036] Note 2: Catalyst molecular weight is 11.5 kg / mol, molecular weight distribution is 1.26.

[0037] Among them, if the yield of cyclohexene oxide is low, the yield can be further increased by adjusting the reaction conditions.

[0038] Example 2

[0039] A cyclic catalytic pyrolysis recovery test of catalytic pyrolysis polycarbonate plastic

[0040]

[0041] First cycle: Porphyrin chromium (Cr III -TPP, 10 mg, 1 equiv.), bis(triphenylphosphine)ammonium azide (PPN-N3, 8 mg, 1 equiv.) and polycyclohexene carbonate (PCHC, 1.1 g, 500 equiv.) were placed in a 25 mL Schulink bottle and dissolved with 1 mL of dichloromethane, then the solvent was removed under reduced pressure and the Schulink bottle was closed. The residue was heated at 200 ° C for 20 minutes. After cooling to room temperature, a small amount of brown liquid was taken and tested by nuclear magnetic resonance analysis to calculate the conversion rate of polycyclohexene carbonate and the distribution of degradation products.

[0042] Second cycle: Then add new polycyclohexene carbonate (1.1 g, 500 equiv.) to the residue, add 1 mL of dichloromethane, remove the solvent under reduced pressure and close the Schulink bottle. Heat the residue at 200 ° C for 20 minutes. After cooling to room temperature, take a small amount of brown liquid and test it by NMR analysis to calculate the PCHC conversion rate and degradation product distribution.

[0043] The third cycle is the same as the second cycle.

[0044] The catalytic system composed of porphyrin chromium and bis(triphenylphosphine)ammonium azide still maintains a conversion rate and selectivity of 99% after three cycles of catalytic degradation of polycarbonate.

[0045] Example 3

[0046] The method for selectively recovering polycarbonate in a defined polymer mixture is carried out as follows:

[0047] Porphyrin chromium catalyst (49 mg, 1 equiv.), bis(triphenylphosphine) ammonium azide (PPN-N3, 41 mg, 1 equiv.), polycyclohexene carbonate (PCHC, 5.0 g, 500 equiv.), polypropylene (1 g), high-density polyethylene (1 g), polyethylene terephthalate (1 g), and polylactic acid (1 g) were placed in a 100 mL flask, completely dissolved with 10 mL of dichloromethane, and then the solvent was removed under reduced pressure. Using a vacuum distillation apparatus, the PCHC mixture was heated to 200°C under negative pressure conditions for 20 min, and the distillate in the receiving bottle was collected. The reaction was stopped, and after cooling for 10 minutes, 3.2 g (93% yield) of liquid was recovered. No PCHC solid residue was detected by nuclear magnetic resonance, and the monomer purity reached 99% by gas phase detection.

Claims

1. A method for catalytic pyrolysis of polycarbonate plastics, characterized in that: Under negative pressure conditions with a reaction temperature of 100 to 250°C and no solvent, polycarbonate plastic is directly degraded into alkylene oxide monomers and carbon dioxide using a catalyst; the molar ratio of the catalyst to the repeating unit in the polycarbonate in the catalytic pyrolysis reaction system is 1: 10~1:5000, reaction time is 0.1~24 hours; in, The catalyst is a metal complex catalyst 1 with a porphyrin structure as a skeleton or a metal complex catalyst 2 with a phthalocyanine structure as a skeleton; the structural formulas of the two are as follows: in, M=Cr,Al; M1=Cr, Al, Mg, Zn, Cu; The polycarbonate plastic is suitable for alicyclic polycarbonate with a molecular weight of 1 to 1000 kg / mol and a molecular weight distribution of 1.0 to 5.0, and the structure is as follows:

2. The method according to claim 1, characterized in that Adding co-catalyst R into the reaction system 1 R 2 3YX 1 , where R 1 R 2 3 is the cationic part of the cocatalyst, which is tetramethyl, tetraethyl, tetrabutyl, tetrapropyl, benzyltriethyl, benzyltripropyl, benzyltributyl, hexadecyltrimethyl, dodecyltrimethyl, bis-(triphenylphosphorane), butyltriphenyl, benzyltriphenyl or propyltriphenyl, and Y is nitrogen or phosphorus; X 1 Cl -1 Br -1 ,I -1 、NO3 -1 、CH3COO -1 、ClO4 -1 、BF4 -1 OH -1 ,BPh4 -1 or N3 -1 Monovalent anion; the molar ratio of the co-catalyst to the catalyst is not greater than 10.

3. The method according to claim 1, characterized in that Other polymer materials also exist in the reaction system.

4. The method according to claim 3, characterized in that The polymer materials include double A polycarbonate, polystyrene, polypropylene, high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polyamide, polyethylene terephthalate, polyhydroxyalkanoate, and polylactic acid.