Organic silicon pressure-sensitive adhesive with stable adhesion in medium and high adhesion range, preparation method and application thereof

By using POSS and other ingredients formulas in silicone pressure-sensitive adhesives, a stable crosslinking network is formed, which solves the problem of unstable adhesion within the medium and high adhesion range, and achieves stable application in the field of high-end process protection.

CN116218456BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310000461.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-12-03
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

The existing silicone pressure-sensitive adhesive with medium and high adhesion range has defects in adhesion stability, making it difficult to achieve stability within the range of 100-400gf, resulting in large fluctuations in adhesion during use, which cannot meet the needs of high-end process protection. .

Method used

The formulations of POSS, methylvinyl silicone rubber raw rubber, hydroxyl raw rubber, methyl MQ silicone resin, vinyl MQ silicone resin, hydrogen silicone crosslinking agent and solvent are adopted to participate in hydrogen silicon crosslinking through alkoxy groups and hydroxyl groups. Form a stable cross-linking network to enhance the adhesion stability of the adhesive film.

Benefits of technology

The adhesive stability within the medium and high adhesive range is achieved, the adhesive unstable problem caused by the combination of traditional high and low adhesive sensitive adhesives is avoided, and stable application in the field of high-end process protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004034248930000031
    Figure BDA0004034248930000031
  • Figure BDA0004034248930000041
    Figure BDA0004034248930000041
  • Figure BDA0004034248930000131
    Figure BDA0004034248930000131
Patent Text Reader

Abstract

The present invention discloses an organosilicon pressure-sensitive adhesive with stable adhesion in a medium-high adhesion range, which comprises hydroxyl and alkoxy cage-type polysilsesquioxane (POSS) functional additives, vinyl silicone rubber with different vinyl contents, hydroxyl raw rubber, methyl MQ silicone resin, vinyl MQ silicone resin, inhibitors, and solvents. The present invention plays a certain crosslinking and toughening role by adding POSS additives with customized functional groups, so that the pressure-sensitive adhesive film has stable adhesion in a medium-high adhesion range, achieving excellent performance that exceeds the performance of industry competitors. The prepared organosilicon pressure-sensitive adhesive can meet the stringent requirements of a narrow fluctuation range in a medium-high adhesion range in related fields such as high-end process protective films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organosilicon pressure-sensitive materials, and in particular to an organosilicon pressure-sensitive adhesive having stable adhesion in a medium-high adhesion range and small adhesion fluctuation over time, and a preparation method thereof. Background Art

[0002] Silicone pressure-sensitive adhesive is a special silicone system adhesive. When it is attached to the surface of the adherend, it can provide good adhesion by applying a certain pressure. The pressure-sensitive adhesive and the surface of the adherend will form a good interface interaction, which is contributed by various forces such as van der Waals force, hydrogen bond, acid-base proton pair effect, donor-acceptor effect, etc. Silicone pressure-sensitive adhesive is mainly composed of silicone elastomer rubber (providing mechanical strength), silicone tackifying resin (providing viscosity), catalyst, cross-linking agent, solvent and other additives. The main components and the ones that determine most of the performance of silicone pressure-sensitive adhesive are silicone rubber and MQ silicone resin composed of polysiloxane.

[0003] With the rapid development of electronic and information technology, the demand for protection of components such as circuit boards and display screens has also continued to grow, and the application requirements of process protection films have also continued to increase. Medium-high viscosity silicone pressure-sensitive adhesives usually refer to pressure-sensitive adhesives with a 180° peel force in the range of 100-400gf. Current silicone pressure-sensitive adhesives are usually used in combination with high-viscosity (~1000gf adhesion) and low-viscosity (~1gf) pressure-sensitive adhesives. It is difficult to achieve stability within the adhesion range of 100-400gf, the adhesion curve is uneven, and the adhesion fluctuation range is large; a few suppliers on the market have medium-high viscosity products, which are also difficult to achieve stable adhesion and poor batch-to-batch stability. It is difficult for customers to control when using it, and it is easy to have too high or too low adhesion, which cannot meet the needs of high-end process protection.

[0004] Chinese patent CN112175576A discloses a method for preparing an organic silicon pressure-sensitive adhesive, which is synthesized by using silicone resin, silicone rubber, a cross-linking agent, a solvent, etc., but can only achieve a relatively high adhesion range, and the medium adhesion range has not been studied;

[0005] Chinese patent CN106753195B discloses a method for preparing a silicone pressure-sensitive adhesive and a pressure-sensitive adhesive tape or film, but the invention is blank in the medium-high adhesive force range of 100-400 gf, and fails to achieve stability control in the medium-high adhesive force range;

[0006] Chinese patent CN113956837A discloses a method for synthesizing a high-temperature silicone pressure-sensitive adhesive, which uses vinyl-modified POSS as a functional additive. It only achieves the need for non-pause printing and high anchoring of screen protective films, but does not benefit medium- and high-adhesion process protective films. Summary of the invention

[0007] In order to solve the common defects in the existing medium and high adhesion range, the present invention provides a silicone pressure-sensitive adhesive with stable adhesion in the medium and high adhesion range, which can achieve stable medium adhesion and is applied in the field of process protection; its formula process is relatively simple, which is conducive to large-scale preparation.

[0008] Another object of the present invention is to provide a method for preparing the organosilicon pressure-sensitive adhesive with medium to high adhesion and stability.

[0009] Another object of the present invention is to provide an application of the organic silicone pressure-sensitive adhesive with medium to high adhesion and stability.

[0010] To achieve the above object, the technical solution of the present invention is as follows:

[0011] The invention discloses an organic silicon pressure-sensitive adhesive with stable adhesion in a medium to high adhesion range. The raw materials of the organic silicon pressure-sensitive adhesive include POSS, methyl vinyl silicone rubber raw rubber, hydroxyl raw rubber, methyl MQ silicone resin, vinyl MQ silicone resin, silicon-hydrogen crosslinking agent, inhibitor and solvent.

[0012] Preferably, the formula components include by weight: 100 parts of methyl vinyl silicone rubber raw rubber, 10-70 parts of hydroxyl raw rubber, 100-300 parts of MQ resin, 100-300 parts of solvent, 0.5-1.5 parts of silicon hydrogen crosslinking agent, 0.1-2.0 parts of inhibitor, and 0.2-2.0 parts of POSS; wherein the mass ratio of methyl MQ silicone resin to vinyl MQ silicone resin in the MQ resin is 1:0.2-5.

[0013] In a specific embodiment, the POSS structural formula is as follows:

[0014]

[0015] The R functional groups are independently selected from hydroxyl, methoxy, and ethoxy, preferably the R functional group is hydroxyl or methoxy;

[0016] The present invention adds a POSS additive to participate in silicon-hydrogen crosslinking through alkoxy and hydroxyl groups instead of vinyl groups, which has a toughening effect on the crosslinked network, helps to stabilize the adhesion of the film, and the cured organic silicone pressure-sensitive adhesive has stable peeling force in the medium and high adhesion range, solving the problem of unstable adhesion existing in the previous combination of high and low viscosity pressure-sensitive adhesives.

[0017] The preparation process of described POSS comprises the following steps:

[0018] (1) A certain amount of sodium ethoxide, isopropanol and deionized water are placed in a three-necked flask equipped with a reflux condenser and a magnetic stirrer.

[0019] (2) The flask was sealed with dry nitrogen, a certain amount of orthosilicic acid and alkoxytrimethoxysilane were added dropwise to the reaction mixture, and the mixture was stirred and refluxed at 85±5°C for 5-6 hours, then cooled to room temperature and stirred for another 6-8 hours.

[0020] (3) filtering the precipitate, washing, and drying in a vacuum oven at 65±5°C for 6-8 h to obtain a white powder, which is the target product;

[0021] In the present invention, the amount of sodium ethoxide in step (1) is 0.1% to 1% of the total amount of orthosilicic acid and alkoxytrimethoxysilane in step (2), the amount of isopropanol and deionized water is 100% to 300% of the total amount of orthosilicic acid and alkoxytrimethoxysilane, and the ratio of isopropanol to deionized water is (0.5-2):1;

[0022] In the present invention, the hydroxyl and alkoxy contents in the final product can be controlled by controlling the addition ratio of orthosilicic acid and alkoxytrimethoxysilane in step (2). Preferably, the dosage ratio of orthosilicic acid and alkoxytrimethoxysilane is 1:2-4. The reaction process involved is as follows:

[0023]

[0024] In the organosilicon pressure-sensitive adhesive of the present invention, preferably, the POSS is a mixture of one or two of dihydroxyhexamethoxy cage-type polysilsesquioxane, hydroxyheptamethoxy cage-type polysilsesquioxane, etc.

[0025] In some specific embodiments of the organosilicon pressure-sensitive adhesive of the present invention, the vinyl mass fraction of the methyl vinyl silicone rubber raw rubber is 0.03-1.5%, preferably 0.05-0.5%, and the molecular weight is 500,000-800,000, preferably 600,000-700,000.

[0026] In some specific embodiments of the organosilicon pressure-sensitive adhesive of the present invention, the hydroxyl raw rubber is selected from terminal hydroxyl polydimethylsiloxane (107 raw rubber) with a molecular weight of 500,000-800,000, preferably 600,000-700,000.

[0027] The raw rubber and the POSS additive selected in the present invention form an effective cross-linking network during cross-linking, and the final pressure-sensitive adhesive film has stable adhesion and is not easy to climb or fall.

[0028] In some specific embodiments of the organic silicone pressure-sensitive adhesive of the present invention, the M / Q ratio of the methyl MQ silicone resin is 0.5 to 1.0, and the molar mass is 2700 to 5000 g / mol. The structural formula of the methyl MQ resin is (R3SiO 1 / 2 ) m (SiO 4 / 2 ) n , wherein R is methyl or hydroxyl.

[0029] In some specific embodiments of the organosilicon pressure-sensitive adhesive of the present invention, the M / Q ratio of the vinyl MQ silicone resin is 0.5 to 1.0, the vinyl mass fraction is 0.5 to 2%, and the molar mass is 4000 to 5000 g / mol. The structural formula of the vinyl MQ resin is (R3SiO 1 / 2 ) m (SiO 4 / 2 ) n , wherein R is vinyl or hydroxyl.

[0030] In some specific embodiments of the organosilicon pressure-sensitive adhesive of the present invention, the solvent is selected from any one or a combination of toluene, ester solvents, ketone solvents, and alkane solvents, wherein the ester solvents include, but are not limited to, ethyl acetate, the ketone solvents include, but are not limited to, acetone, and the alkane solvents include, but are not limited to, n-heptane.

[0031] In some specific embodiments of the organosilicon pressure-sensitive adhesive of the present invention, the viscosity of the silicon-hydrogen crosslinking agent is 20-150 mPa.s, and the silicon-hydrogen crosslinking agent is a hydrogen-containing silicone oil (such as H510, H512) containing terminal hydrogen groups and side hydrogen groups and a total hydrogen group mass fraction of 0.7-1.6%.

[0032] In some specific embodiments of the silicone pressure-sensitive adhesive of the present invention, the inhibitor is selected from any one or a combination of tetramethyltetravinylcyclotetrasiloxane, divinyltetramethyldisiloxane, methyl acetylene alcohol, ethynylcyclohexanol, methyl butynol, 3,5-dimethyl-1-hexynyl-3-ol, and 3-methyl-1-dodecyn-3-ol, preferably ethynylcyclohexanol.

[0033] On the other hand, the present invention provides a method for preparing an organosilicon pressure-sensitive adhesive having stable adhesion in a medium to high adhesion range, comprising the following steps:

[0034] 1) Add methyl vinyl silicone rubber raw rubber, hydroxyl raw rubber, methyl MQ silicone resin, vinyl MQ silicone resin, inhibitor, solvent and POSS into a reaction kettle, and start stirring to fully dissolve the raw rubber in the solvent;

[0035] 2) Add nitrogen and stir until evenly mixed, then slowly add 0.05-2% of the catalyst by weight of the methyl vinyl silicone rubber, then heat to 120-150°C, reflux and dehydrate for 3-5 hours until no water is produced;

[0036] Preferably, the catalyst is selected from any one or more of acetic acid, propionic acid, benzoic acid, phenylacetic acid, trifluorobenzenesulfonic acid or acidic diatomaceous earth.

[0037] 3) Cooling to room temperature, adding a silicon hydrogen crosslinking agent, stirring for 1 to 3 hours, and mixing evenly to obtain a silicone pressure-sensitive adhesive with stable adhesion in a medium to high adhesion range.

[0038] The organic silicon pressure-sensitive adhesive is coated and cured to obtain a pressure-sensitive adhesive film.

[0039] In another aspect, the present invention relates to the use of the aforementioned organosilicon pressure-sensitive adhesive with stable adhesion in the medium-to-high adhesion range or the organosilicon pressure-sensitive adhesive prepared by the above preparation method in the field of high-end process protective films.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1) Compared with the traditional organic silicon pressure sensitive adhesive formula, in the present invention, a POSS additive with an alkenyl functional group is added to the pressure sensitive adhesive by physical blending, and when the film is cured under high temperature and the action of a catalyst, the alkoxy group and the hydroxyl group help to react with silicon hydrogen to undergo dealcoholization and dehydrogenation to form a cross-linked network under the action of silicon hydrogen. Different from the commonly used vinyl raw materials, the alkoxy group and the hydroxyl group participate in the reaction together, so as to avoid too fast cross-linking reaction during heat curing, thereby forming a more uniform cross-linked structure, improving the cohesive strength of the adhesive, controlling the hardness of the adhesive surface, and avoiding the unstable initial adhesion during use.

[0042] 2) The silicone pressure-sensitive adhesive prepared by the formula of the present invention can be coated on common 50μm PET, 100μm PET, PI and other substrates, has a relatively stable peeling force on steel plates and glass, and the adhesive surface has good anchoring properties. DETAILED DESCRIPTION

[0043] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0044] Source of raw materials:

[0045] Methyl vinyl silicone rubber raw rubber Wanhua Chemical,

[0046] Hydroxylated rubber Wanhua Chemical,

[0047] MQ resin Wanhua Chemical,

[0048] Toluene analytical grade Inokane,

[0049] Silicon-hydrogen crosslinking agent Wanhua Chemical,

[0050] Inhibitor Wanhua Chemical,

[0051] POSS Wanhua Chemical;

[0052] The performance test method of the prepared silicone pressure-sensitive adhesive is as follows:

[0053] 1. Viscosity test method refers to GB / T 10247-2008;

[0054] 2. The adhesion test method refers to GB / T 2792-1998;

[0055] 3. Adhesion stability tracking method: Place the prepared adhesive film with the protective film in a constant temperature and humidity environment (23°C, 50% RH) and store it. Test the adhesion once a week for 1 month. The adhesion test refers to GB / T2792-1998.

[0056] Example 1

[0057] POSS dihydroxy hexamethoxy cage-type polysilsesquioxane, the preparation method is as follows:

[0058] (1) 0.08 g of sodium ethoxide, 120 g of isopropyl alcohol and 120 g of deionized water were placed in a three-necked flask equipped with a reflux condenser and a magnetic stirrer.

[0059] (2) The flask was sealed with dry nitrogen, 20 g of orthosilicic acid and 60 g of methoxytrimethoxysilane were added dropwise to the reaction mixture, and the mixture was stirred and refluxed at 85°C for 6 h, then cooled to room temperature and stirred for another 6 h.

[0060] (3) filtering the precipitate, washing, and drying in a vacuum oven at 65° C. for 8 h to obtain a white powder, which is the target product and the mixture;

[0061] Methyl vinyl silicone rubber raw rubber: molecular weight 600,000, vinyl mass fraction 0.5%;

[0062] Vinyl MQ silicone resin: M / Q ratio is 0.7, vinyl mass fraction is 1.5%, and molar mass is 4400 g / mol;

[0063] Hydroxylated raw rubber: molecular weight 600,000;

[0064] Methyl MQ silicone resin: M / Q ratio is 0.7, molar mass is 3000 g / mol;

[0065] Silicon-hydrogen crosslinking agent: The viscosity is 100 mPa.s, and the mass fraction of terminal hydrogen groups and side hydrogen groups is 1.6%.

[0066] 1) 15 g of methyl vinyl silicone rubber, 5 g of hydroxyl rubber, 15 g of vinyl MQ silicone resin, 25 g of methyl MQ silicone resin, 35 g of toluene, 0.25 g of POSS, and 0.1 g of ethynyl cyclohexanol inhibitor were added to a reactor and stirred to dissolve;

[0067] 2) nitrogen was introduced and stirred, and after stirring evenly, 0.18 g of acetic acid was diluted with 5 g of toluene and slowly added, and then reacted at 150° C. under reflux and dehydration for 4 h;

[0068] 3) Cool to room temperature, add 0.1 g of silicon hydrogen crosslinking agent and stir evenly to obtain pressure-sensitive adhesive base-1.

[0069] In 20g of base glue-1, add 15g of toluene, stir evenly, add 0.6g of platinum catalyst with a platinum content of 5000ppm, stir evenly, apply it on a 50μm thick PET substrate, place it in an oven at 150℃*2min for curing, and then stick a fluoroplastic protective film. Peel off the fluoroplastic protective film to test the performance, the results are shown in Table 1.

[0070] Example 2

[0071] POSS: hydroxyheptaethoxy cage polysilsesquioxane, ethoxy cage polysilsesquioxane;

[0072] (1) 0.08 g of sodium ethoxide, 120 g of isopropyl alcohol and 120 g of deionized water were placed in a three-necked flask equipped with a reflux condenser and a magnetic stirrer.

[0073] (2) The flask was sealed with dry nitrogen, 10 g of orthosilicic acid and 70 g of ethoxytrimethoxysilane were added dropwise to the reaction mixture, and the mixture was stirred and refluxed at 90° C. for 6 h, then cooled to room temperature and stirred for another 6 h.

[0074] (3) filtering the precipitate, washing, and drying in a vacuum oven at 70° C. for 6 h to obtain a white powder, which is the target product and the mixture;

[0075] Methyl vinyl silicone rubber raw rubber: molecular weight 700,000, vinyl mass fraction 0.1%;

[0076] Vinyl MQ silicone resin: M / Q ratio is 0.7, vinyl mass fraction is 0.5%, and molar mass is 4800 g / mol;

[0077] Hydroxylated raw rubber: molecular weight 700,000;

[0078] Methyl MQ silicone resin: M / Q ratio is 0.7, molar mass is 5000 g / mol;

[0079] Silicon-hydrogen crosslinking agent: The viscosity is 100 mPa.s, and the mass fraction of terminal hydrogen groups and pendant hydrogen groups is 1.0%.

[0080] 1) 33 g of methyl vinyl silicone rubber, 4 g of hydroxyl rubber, 15 g of vinyl MQ silicone resin, 20 g of methyl MQ silicone resin, 35 g of ethyl acetate, 0.6 g of POSS, and 0.3 g of divinyltetramethyldisiloxane inhibitor were added to a reaction kettle and stirred to dissolve;

[0081] 2) nitrogen was introduced and stirred, and after stirring evenly, 0.15 g of benzoic acid was diluted with 5 g of ethyl acetate and slowly added, and then reacted under reflux dehydration at 120° C. for 3 h;

[0082] 3) Cool to room temperature, add 0.2 g of silicon hydrogen crosslinking agent and stir evenly to obtain pressure-sensitive adhesive base glue-2.

[0083] In 20g of base glue-2, add 15g of ethyl acetate, stir evenly, add 0.6g of platinum catalyst with a platinum content of 5000ppm, stir evenly, apply it on a 80μm thick PET substrate, place it in an oven at 150℃*2min for curing, and then stick a PET protective film. Peel off the PET protective film to test the performance, the results are shown in Table 1.

[0084] Example 3

[0085] POSS: dihydroxyhexaethoxy cage-type polysilsesquioxane;

[0086] (1) 0.08 g of sodium ethoxide, 120 g of isopropyl alcohol and 120 g of deionized water were placed in a three-necked flask equipped with a reflux condenser and a magnetic stirrer.

[0087] (2) The flask was sealed with dry nitrogen, 20 g of orthosilicic acid and 60 g of ethoxytrimethoxysilane were added dropwise to the reaction mixture, and the mixture was stirred and refluxed at 80° C. for 6 h, then cooled to room temperature and stirred for another 7 h.

[0088] (3) filtering the precipitate, washing, and drying in a vacuum oven at 60° C. for 7 h to obtain a white powder, which is the target product;

[0089] Methyl vinyl silicone rubber raw rubber: molecular weight 500,000, vinyl mass fraction 0.4%;

[0090] Vinyl MQ silicone resin: M / Q ratio is 0.7, vinyl mass fraction is 1.8%, and molar mass is 4000 g / mol;

[0091] Hydroxylated raw rubber: molecular weight 500,000;

[0092] Methyl MQ silicone resin: M / Q ratio is 0.7, molar mass is 3000 g / mol;

[0093] Silicon-hydrogen crosslinking agent: The viscosity is 80 mPa.s, and the mass fraction of terminal hydrogen groups and side hydrogen groups is 0.8%.

[0094] 1) 20 g of methyl vinyl silicone rubber, 10 g of hydroxyl rubber, 20 g of methyl MQ silicone resin, 10 g of vinyl MQ silicone resin, 35 g of toluene, 0.3 g of POSS, and 0.1 g of ethynyl cyclohexanol inhibitor were added to a reactor and stirred to dissolve;

[0095] 2) nitrogen was introduced and stirred, and after stirring evenly, 0.2 g of propionic acid was diluted with 5 g of toluene and slowly added, and then reacted at 150° C. under reflux and dehydration for 5 h;

[0096] 3) Cool to room temperature, add 0.2 g of silicon hydrogen crosslinking agent and stir evenly to obtain pressure-sensitive adhesive base-3.

[0097] In 20g of base glue-3, add 15g of toluene, stir evenly, add 0.5g of platinum catalyst with a platinum content of 5000ppm, stir evenly, apply it on a 50μm thick PET substrate, place it in an oven at 150℃*2min for curing, and then attach the PET protective film. Remove the PET protective film to test the performance, the results are shown in Table 1.

[0098] Example 4

[0099] POSS: hydroxyheptamethoxy cage-type polysilsesquioxane;

[0100] (1) 0.08 g of sodium ethoxide, 120 g of isopropyl alcohol and 120 g of deionized water were placed in a three-necked flask equipped with a reflux condenser and a magnetic stirrer.

[0101] (2) The flask was sealed with dry nitrogen, 10 g of orthosilicic acid and 70 g of methoxytrimethoxysilane were added dropwise to the reaction mixture, and the mixture was stirred and refluxed at 85° C. for 5 h, then cooled to room temperature and stirred for another 8 h.

[0102] (3) filtering the precipitate, washing, and drying in a vacuum oven at 65° C. for 8 h to obtain a white powder, which is the target product and the mixture;

[0103] Methyl vinyl silicone rubber raw rubber: molecular weight 600,000, vinyl mass fraction 0.5%;

[0104] Vinyl MQ silicone resin: M / Q ratio is 0.7, vinyl mass fraction is 1.5%, and molar mass is 4400 g / mol;

[0105] Hydroxylated raw rubber: molecular weight 600,000;

[0106] Methyl MQ silicone resin: M / Q ratio is 0.7, molar mass is 4500 g / mol;

[0107] Silicon-hydrogen crosslinking agent: The viscosity is 80 mPa.s, and the mass fraction of terminal hydrogen groups and side hydrogen groups is 0.8%.

[0108] 1) 20 g of methyl vinyl silicone rubber, 5 g of hydroxyl rubber, 25 g of methyl MQ silicone resin, 10 g of vinyl MQ silicone resin, 35 g of toluene, 0.1 g of POSS, and 0.4 g of methyl acetylene alcohol inhibitor were added to a reactor and stirred to dissolve;

[0109] 2) nitrogen was introduced and stirred, and after stirring evenly, 0.18 g of propionic acid was diluted with 20 g of toluene and slowly added, and then reacted under reflux dehydration at 130° C. for 5 h;

[0110] 3) Cool to room temperature, add 0.3 g of silicon hydrogen crosslinking agent and stir evenly to obtain pressure-sensitive adhesive base glue-4.

[0111] In 20g of base glue-4, add 15g of toluene, stir evenly, add 0.5g of platinum catalyst with a platinum content of 5000ppm, stir evenly, apply it on a 25μm thick PI substrate, place it in an oven at 150℃*2min for curing, and then stick a fluorine protective film. Peel off the fluorine protective film to test the performance, the results are shown in Table 1.

[0112] Comparative Example 1

[0113] POSS: vinyl cage polysilsesquioxane (purchased from Hybrid Plastic Company);

[0114] Methyl vinyl silicone rubber raw rubber: molecular weight 600,000, vinyl mass fraction 0.5%;

[0115] Vinyl MQ silicone resin: M / Q ratio is 0.7, vinyl mass fraction is 1.5%, and molar mass is 4400 g / mol;

[0116] Hydroxylated raw rubber: molecular weight 600,000;

[0117] Methyl MQ silicone resin: M / Q ratio is 0.7, molar mass is 3000 g / mol;

[0118] Silicon-hydrogen crosslinking agent: The viscosity is 100 mPa.s, and the mass fraction of terminal hydrogen groups and side hydrogen groups is 1.6%.

[0119] 1) 15 g of methyl vinyl silicone rubber, 5 g of hydroxyl rubber, 15 g of vinyl MQ silicone resin, 25 g of methyl MQ silicone resin, 35 g of toluene, 0.25 g of POSS, and 0.1 g of ethynyl cyclohexanol inhibitor were added to a reactor and stirred to dissolve;

[0120] 2) nitrogen was introduced and stirred, and after stirring evenly, 0.18 g of acetic acid was diluted with 5 g of toluene and slowly added, and then reacted at 150° C. under reflux and dehydration for 4 h;

[0121] 3) Cool to room temperature, add 0.1 g of silicon hydrogen crosslinking agent and stir evenly to obtain pressure-sensitive adhesive base-1.

[0122] In 20g of base glue-1, add 15g of toluene, stir evenly, add 0.6g of platinum catalyst with a platinum content of 5000ppm, stir evenly, apply it on a 50μm thick PET substrate, place it in an oven at 150℃*2min for curing, and then stick a fluoroplastic protective film. Peel off the fluoroplastic protective film to test the performance, the results are shown in Table 1.

[0123] Comparative Example 2: Traditional pressure-sensitive adhesive without adding additional additives

[0124] Methyl vinyl silicone rubber raw rubber: molecular weight 700,000, vinyl mass fraction 0.1%;

[0125] Vinyl MQ silicone resin: M / Q ratio is 0.7, vinyl mass fraction is 0.5%, and molar mass is 4800 g / mol;

[0126] Hydroxylated raw rubber: molecular weight 700,000;

[0127] Methyl MQ silicone resin: M / Q ratio is 0.7, molar mass is 5000 g / mol;

[0128] Silicon-hydrogen crosslinking agent: The viscosity is 100 mPa.s, and the mass fraction of terminal hydrogen groups and pendant hydrogen groups is 1.0%.

[0129] 1) 33 g of methyl vinyl silicone rubber, 24 g of hydroxyl rubber, 515 g of vinyl MQ silicone resin, 20 g of methyl MQ silicone resin, 35 g of ethyl toluene acetate, and 0.3 g of divinyltetramethyldisiloxane inhibitor were added to a reaction kettle and stirred to dissolve;

[0130] 2) nitrogen was introduced and stirred, and after stirring evenly, 0.15 g of benzoic acid was diluted with 5 g of ethyl acetate and slowly added, and then reacted under reflux dehydration at 120° C. for 3 h;

[0131] 3) Cool to room temperature, add 0.2 g of silicon hydrogen crosslinking agent and stir evenly to obtain pressure-sensitive adhesive base glue-2.

[0132] In 20g of base glue-2, add 15g of ethyl acetate, stir evenly, add 0.6g of platinum catalyst with a platinum content of 5000ppm, stir evenly, apply it on a 80μm thick PET substrate, place it in an oven at 150℃*2min for curing, and then stick a PET protective film. Peel off the PET protective film to test the performance, the results are shown in Table 1.

[0133] The test performance data of the silicone pressure-sensitive adhesives prepared in the above embodiments and comparative examples are shown in Table 1 below:

[0134] Table 1 Performance of silicone pressure-sensitive adhesives of Examples 1-4 and Comparative Examples

[0135]

[0136]

[0137] As can be seen from the table, in the present invention, by physical blending, increase the POSS additive with hydroxyl or alkoxy functional group in pressure-sensitive adhesive, when solidifying into film under high temperature, catalyst action, wherein hydroxyl or alkoxy helps to form stable cross-linked network structure under silicon hydrogen effect, the cross-linked POSS structure plays a cross-linking density stabilization and toughening effect, making conventional organosilicon pressure-sensitive adhesive difficult to do stable medium and high adhesive force scope can accomplish more stable adhesive force equally. The organosilicon pressure-sensitive adhesive that the present invention's formula makes can be coated on substrates such as common 50um PET, 100um PET, 25um PI, can obtain more stable adhesive force.

[0138] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A silicone pressure-sensitive adhesive comprising, by weight: 100 parts of methyl vinyl silicone rubber raw rubber, 10-70 parts of hydroxyl raw rubber, 100-300 parts of MQ resin, 100-300 parts of solvent, 0.5-1.5 parts of silane crosslinking agent, 0.1-2.0 parts of inhibitor, and 0.2-2.0 parts of POSS; wherein the mass ratio of methyl MQ silicone resin to vinyl MQ silicone resin in the MQ resin is 1:0.2-5; the structural formula of the POSS is as follows: The R functional groups are independently selected from hydroxyl, methoxy, and ethoxy.

2. The organic silicone pressure-sensitive adhesive according to claim 1, characterized in that: The R functional group in the POSS structural formula is a hydroxyl group or a methoxy group.

3. The organic silicone pressure-sensitive adhesive according to claim 1, characterized in that: The POSS is one or more of dihydroxyhexamethoxy cage-type polysilsesquioxane, hydroxyheptamethoxy cage-type polysilsesquioxane, and dihydroxyhexamethoxy cage-type polysilsesquioxane.

4. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The vinyl mass fraction of the methyl vinyl silicone rubber raw rubber is 0.03-1.5%, and the molecular weight is 500,000-800,000.

5. The organic silicone pressure-sensitive adhesive according to claim 4, characterized in that: The vinyl mass fraction of the methyl vinyl silicone rubber raw rubber is 0.05-0.5%, and the molecular weight is 600,000-700,000.

6. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The M / Q ratio of the methyl MQ silicone resin is 0.5-1.0, and the molar mass is 2700-5000 g / mol; and / or the M / Q ratio of the vinyl MQ silicone resin is 0.5-1.0, the vinyl mass fraction is 0.5-2%, and the molar mass is 4000-5000 g / mol.

7. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The solvent is selected from at least one of toluene, ester solvents, ketone solvents and alkane solvents.

8. The organic silicone pressure-sensitive adhesive according to claim 7, characterized in that: The ester solvent includes ethyl acetate, the ketone solvent includes acetone, and the alkane solvent includes heptane.

9. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The viscosity of the silicon-hydrogen crosslinking agent is 20-150 mPa.s, and the agent is a hydrogen-containing silicone oil containing terminal hydrogen groups and side hydrogen groups, with a total hydrogen group mass fraction of 0.7-1.6%.

10. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The inhibitor is selected from at least one of tetramethyltetravinylcyclotetrasiloxane, divinyltetramethyldisiloxane, methylacetylene alcohol, ethynylcyclohexanol, methylbutynol, 3,5-dimethyl-1-hexynyl-3-ol, and 3-methyl-1-dodecyn-3-ol.

11. The method for preparing the organosilicon pressure-sensitive adhesive according to any one of claims 1 to 10, characterized in that: The following steps are involved: 1) Add methyl vinyl silicone rubber raw rubber, hydroxyl raw rubber, methyl MQ silicone resin, vinyl MQ silicone resin, inhibitor, solvent and POSS into a reaction kettle, and start stirring to fully dissolve the raw rubber in the solvent; 2) Add nitrogen and stir until evenly mixed, then slowly add 0.05-2% of the catalyst by weight of the methyl vinyl silicone rubber, then heat to 120-150°C, reflux and dehydrate for 3-5 hours until no water is produced; 3) Cooling to room temperature, adding a silicon hydrogen crosslinking agent, stirring for 1 to 3 hours, and mixing evenly to obtain a silicone pressure-sensitive adhesive with stable adhesion in a medium to high adhesion range.

12. Use of the organosilicon pressure-sensitive adhesive according to any one of claims 1 to 10 or the organosilicon pressure-sensitive adhesive prepared by the preparation method according to claim 11 in the field of high-end process protective films.

Citation Information

Patent Citations

  • An organosilicon pressure-sensitive adhesive and pressure-sensitive adhesive tape or film

    CN106753195B

  • Organic silicon pressure-sensitive adhesive

    CN112175576A

  • Organic silicon pressure-sensitive adhesive without pause marks and with high anchoring property, preparation method and application thereof