Optical fiber preform preparation device and method
By completing the deposition, dehydration, sintering, and annealing of optical fiber preforms within a single reaction chamber, the problems of transportation scratches and temperature variations during the production process of optical fiber preforms have been solved, enabling the preparation of high-quality optical fiber preforms.
Patent Information
- Application Number
- CN202080102910.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-10-19
AI Technical Summary
In the current optical fiber preform production process, there are problems such as scratches during transportation, impurity adhesion, and cracking caused by temperature changes, which affect the quality and performance of optical fiber products.
An optical fiber preform fabrication apparatus is provided, comprising a reaction chamber, a clamping mechanism, and a driving mechanism. Deposition, dehydration, sintering, and annealing are completed in one reaction chamber using the VAD method, avoiding the need for the optical fiber preform to be moved between different devices. A partition is used to divide the chamber into multiple chambers for different processing.
This improves the purity and production efficiency of optical fiber preforms, avoids defects caused by impurity adhesion and sudden temperature changes, and enhances the loss performance and strength of optical fibers.
Smart Images

Figure CN116234779B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of optical fiber production, for example, to a device and method for preparing an optical fiber preform. Background Art
[0002] As competition in the optical fiber market becomes increasingly fierce, the market's requirements for optical fiber quality are getting higher and higher. In the optical fiber production process, the quality of optical fiber preform directly affects the performance and parameter indicators of optical fiber products.
[0003] Optical fiber preform production is generally divided into two preparation processes:
[0004] One is to prepare the core rod and the outer cladding separately, and then match the corresponding outer cladding or core rod according to the parameters of the core rod or the outer cladding. Common process methods include the Rod in Cylinder (RIC) process. The advantage of this type of preparation process is that it can prepare large-diameter optical fiber preforms, but there may be parameter mismatches in the process of combining the core rod and the outer cladding, impurities may be introduced in the combination process, and scratches may occur during transportation or combination.
[0005] Another method is to first prepare a loose body of optical fiber preform (also known as loose body, soot body), and then sinter the loose body of optical fiber preform into an optical fiber preform through a sintering process. Common processes include modified chemical vapor deposition (MCVD), axial vapor deposition (VAD) and outside vapor deposition (OVD). This type of preparation process avoids the problem of optical fiber preform being easily scratched during transportation, but in the production process, different processes such as deposition and sintering require the optical fiber preform to be operated between different devices. During the transportation process, due to contact with the outside air and sudden changes in ambient temperature, the optical fiber preform may have impurities attached or cracks due to stress changes during temperature changes, which seriously affects the quality of subsequent optical fiber products and is not conducive to reducing optical fiber loss and improving optical fiber strength. Summary of the invention
[0006] The present invention provides a device and method for preparing an optical fiber preform. The device can prepare an optical fiber preform based on a VAD method. During the preparation process, there is no need to move the optical fiber preform between different devices, thereby improving the quality of the optical fiber preform and significantly improving production efficiency.
[0007] The present disclosure provides a preparation device for an optical fiber preform rod, comprising a reaction chamber, a clamping mechanism and a driving mechanism, wherein the clamping mechanism is arranged in the reaction chamber and is arranged to fix a target rod, and the driving mechanism is arranged to drive the clamping mechanism to rotate around a vertical axis and move up and down in a vertical direction;
[0008] A plurality of partitions are arranged in the reaction chamber, and the plurality of partitions divide the reaction chamber into a first chamber, a second chamber and a third chamber arranged in sequence from bottom to top;
[0009] The partition has a through hole, and the through hole is coaxially arranged with the target rod, so that the target rod can be placed in the first chamber, the second chamber or the third chamber after moving in the vertical direction;
[0010] The first chamber is configured to deposit on the target rod using a VAD method to form a loose body;
[0011] The second chamber is configured to perform a dehydration process and a sintering process on the loose body to obtain an optical fiber preform;
[0012] The third chamber is configured to perform an annealing process on the optical fiber preform.
[0013] A method for preparing an optical fiber preform using the above optical fiber preform preparation device is also provided, the method comprising:
[0014] placing the target rod in the first chamber, and depositing a loose body on the target rod using a VAD method in the first chamber;
[0015] Lifting the target rod, and performing dehydration and sintering treatments on the loose body in the second chamber to obtain an optical fiber preform;
[0016] The optical fiber preform is continuously lifted, and the optical fiber preform in the third chamber is annealed. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a schematic structural diagram of an optical fiber preform preparation device in an embodiment of the present invention;
[0018] Figure 2 is a schematic diagram of the matching structure of a partition made of a rigid material and an optical fiber preform in an embodiment of the present invention;
[0019] Figure 3 It is a schematic diagram of the matching structure between the partition made of flexible material and the optical fiber preform in an embodiment of the present invention.
[0020] In the figure:
[0021] 1. Reaction chamber; 11. First chamber; 12. Second chamber; 121. Sintering chamber; 122. Dehydration chamber; 13. Third chamber;
[0022] 2. Card holding mechanism;
[0023] 3. Driving mechanism; 31. First power assembly; 311. Screw rod; 312. Support member; 313. Synchronous pulley mechanism; 314. First motor; 32. Second power assembly; 321. Lifting seat; 322. Second motor;
[0024] 4. Target stick;
[0025] 5. partition; 51. first partition; 52. second partition; 53. third partition;
[0026] 6. Blowtorch;
[0027] 7. Control system;
[0028] 10. Optical fiber preform. DETAILED DESCRIPTION
[0029] The present disclosure is described below in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are only used to illustrate the present disclosure.
[0030] In the description of the present disclosure, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. The specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.
[0031] In the present disclosure, unless otherwise expressly specified and limited, a first feature being “above” or “below” a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being “above”, “above”, and “above” a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0032] In the description of this embodiment, the terms "upper", "lower", "right" and other directions or positional relationships are based on the directions or positional relationships shown in the drawings, and are only for the convenience of description and simplified operation, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operate in a specific direction, and therefore cannot be understood as a limitation of the present disclosure. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.
[0033] See also Figure 1 , this embodiment provides a preparation device for an optical fiber preform, which comprises a reaction chamber 1, a holding mechanism 2 and a driving mechanism 3. The holding mechanism 2 is disposed in the reaction chamber 1 and is configured to fix a target rod 4, and the driving mechanism 3 is configured to drive the holding mechanism 2 to rotate around a vertical axis and move up and down in a vertical direction. A plurality of partitions 5 are disposed in the reaction chamber 1, and the plurality of partitions 5 divide the reaction chamber 1 into a first chamber 11, a second chamber 12 and a third chamber 13 arranged sequentially from bottom to top; the partition 5 has a through hole, and the through hole is coaxially disposed with the target rod 4, so that the target rod 4 can be placed in the first chamber 11, the second chamber 12 or the third chamber 13 after moving in the vertical direction, wherein:
[0034] The first chamber 11 is configured to deposit a loose body on the target rod 4 using a VAD method;
[0035] The second chamber 12 is configured to perform a dehydration process and a sintering process on the loose body to obtain an optical fiber preform 10;
[0036] The third chamber 13 is configured to perform an annealing process on the optical fiber preform 10 .
[0037] Deposition: The process by which the raw materials of optical fiber react chemically under certain conditions to form doped quartz glass;
[0038] Sintering: The process of gradually sintering the deposited hollow glass tube into a solid glass rod under a certain heat source. With the above structure, the preparation device completes the deposition, dehydration, sintering and annealing process of the optical fiber preform 10 through a reaction chamber 1, and directly produces the finished glass optical fiber preform 10. Since the optical fiber preform 10 does not need to be operated between different devices during the preparation process, it can avoid the optical fiber preform 10 from contacting with the outside air and adhering impurities, thereby improving the doping purity of the optical fiber preform 10. At the same time, it can also avoid the sudden temperature change of the optical fiber preform 10 caused by transportation, minimize the internal stress caused by the temperature change of the optical fiber preform 10 during the process, and avoid problems such as cracking of the rod. For example, it can be used to manufacture ultra-low loss optical fiber, high-strength optical fiber and special optical fiber.
[0039] In this embodiment, the reaction chamber 1 can be substantially in the form of a hollow cylinder, and a heating device (not shown in the figure) and a temperature sensor (not shown in the figure) are arranged inside the reaction chamber 1 to provide a high temperature environment suitable for the preparation of the optical fiber preform 10. A circulating water pipeline (not shown in the figure) can be arranged outside the reaction chamber 1 to meet the cooling requirements. A chamber cover (not shown in the figure) that can seal or open the reaction chamber 1 is arranged on the top of the reaction chamber 1 to allow the target rod 4 to move into the reaction chamber 1, or to allow the target rod 4 to carry the optical fiber preform 10 out of the reaction chamber 1.
[0040] A blowtorch 6 is arranged in the first chamber 11, and the blowtorch 6 includes a core rod deposition lamp and a cladding deposition lamp. A feeding system (not shown in the figure) connected from the outside of the reaction chamber 1 to the first chamber 11 can provide high-purity SiCl4 and other dopants to the first chamber 11. At the same time, a gas distribution system (not shown in the figure) connected to the first chamber 11, the second chamber 12 and the third chamber 13 can provide inert gas to the first chamber 11, the second chamber 12 and the third chamber 13, thereby forming an inert atmosphere in the first chamber 11, the second chamber 12 and the third chamber 13.
[0041] The clamping mechanism 2 includes a chuck, which is configured to fix the target rod 4 .
[0042] The driving mechanism 3 includes a first power assembly 31 and a second power assembly 32. The first power assembly 31 includes a screw rod 311 extending from the top of the reaction chamber 1 into the third chamber 13 in the vertical direction, the lower end of the screw rod 311 is rotatably connected to a support 312 fixed to the chamber wall of the reaction chamber 1 corresponding to the third chamber 13, and the upper end of the screw rod 311 is transmission-connected to a synchronous pulley mechanism 313, and the synchronous pulley mechanism 313 is driven by a first motor 314. In one embodiment, the screw rod 311 can also be located outside the chamber. The second power assembly 32 includes a lifting seat 321 screwed to the screw rod 311, and a second motor 322 fixed to the lifting seat 321, wherein the lifting seat 321 is arranged to be movable only in the vertical direction, the second motor 322 is arranged so that the rotating shaft is parallel to the vertical direction, and the end of the rotating shaft of the second motor 322 is fixed to the chuck. Through the above structure, the driving mechanism 3 can drive the chuck to rotate around the vertical axis and move up and down in the vertical direction, so that the target rod 4 is placed in the first chamber 11, the second chamber 12 or the third chamber 13.
[0043] The above structures of the clamping mechanism 2 and the driving mechanism 3 are only used as examples in this embodiment. Mechanisms with the same or similar technical effects can be configured based on relevant technologies and are not limited here.
[0044] In this embodiment, the preparation device further includes a control system 7, which includes a control module and an information acquisition module. The control module includes a programmable logic controller (PLC) controller and an operation console. The information acquisition module includes a position sensor (not shown in the figure) and an online monitoring device (not shown in the figure, which may include a temperature sensor, a flow meter, a laser rangefinder, etc.) arranged in the first chamber 11, the second chamber 12 and / or the third chamber 13. The information acquisition module can provide the collected information such as the position of the end of the loose body, the running speed, the running distance, the diameter of the optical fiber preform 10, the transmittance of the optical fiber preform 10, the deposition feeding amount, the hydrogen-oxygen flame gas flow rate of the blowtorch 6 to the control module, and the control module can then adjust the start and stop and the running state of the components such as the heating device, the feeding system, the gas distribution system, the blowtorch 6 and the driving mechanism 3 in the preparation device by means of the above information, so as to control the deposition amount of the loose body and the temperature of the sintering chamber, etc., so as to realize the linkage and conversion of the deposition and sintering processes in the preparation process of the optical fiber preform 10.
[0045] In the above-mentioned control system 7, the control module and the information acquisition module have been used in the preparation equipment for preparing the optical fiber preform 10 using the VAD method, so the components and circuit / communication structure used by the control system 7 will not be described in detail here. In the preparation process performed by the preparation device provided in this embodiment, the specific information collection and processing process required by the control system 7 will be explained in the case below.
[0046] See also Figure 3 In this embodiment, the partition 5 can be made of a rigid material such as metal, and the aperture of the through hole on each partition 5 is correspondingly smaller than the diameter of the loose body or optical fiber preform 10, so that the partition 5 and the loose body or optical fiber preform 10 are interference-fitted. In one embodiment, the aperture of the through hole on the first partition 51 is smaller than the diameter of the loose body, the aperture of the through hole on the second partition 52 is smaller than the diameter of the optical fiber preform 10, and the aperture of the through hole on the third partition 53 is smaller than the diameter of the optical fiber preform 10.
[0047] When the loose body / optical fiber preform 10 is in two or even three chambers at the same time, for example, when the upper half of the loose body is in the second chamber 12 and the lower half is in the first chamber 11, at this time, the first partition 51 located between the first chamber 11 and the second chamber 12 is tightly abutted against the loose body, so that the first chamber 11 and the second chamber 12 are blocked to form an independent atmosphere environment, so that the loose body in the first chamber 11 can continue to be deposited at the bottom of the first chamber 11, while the loose body in the second chamber 12 can be dehydrated or sintered.
[0048] The flexible partition 5 can be made of ceramic fiber, which has the characteristics of high temperature resistance, low thermal conductivity, light bulk density, long service life, high tensile strength, good elasticity and non-toxicity. It does not produce volatile substances when heated and does not affect the quality of the optical fiber preform 10.
[0049] In one embodiment, when the partition 5 is made of flexible material, the difference between the diameter of the optical fiber preform 10 and the aperture of the through hole may be less than 3 mm to ensure that the loose body / optical fiber preform 10 can pass through the through hole smoothly.
[0050] See also Figure 2 In an optional embodiment, the partition 5 can also be made of a flexible material, and there is a preset gap between the through hole on each partition 5 and the loose body or optical fiber preform 10, so as to ensure that the deposited loose body does not scratch the first partition 51 when passing through the first partition 51 between the first chamber 11 and the second chamber 12; and at the same time, ensure that the optical fiber preform 10 obtained by sintering does not scratch the second partition 52 when passing through the second partition 52 between the second chamber 12 and the third chamber 13. The preset gap can be 1-3mm. In one embodiment, the through hole on each partition 5 has a preset gap with the loose body or optical fiber preform 10, which can be: the through hole on the first partition 51 has a preset gap with the loose body, the through hole on the second partition 52 has a preset gap with the optical fiber preform 10, and the through hole on the third partition 53 has a preset gap with the optical fiber preform 10.
[0051] In one embodiment, since the diameter of the loose body / optical fiber preform 10 will change during the deposition, dehydration and sintering processes, the aperture of the through hole provided on each partition 5 can be adjusted accordingly instead of having the same aperture.
[0052] In addition, when the partition 5 is made of a rigid material, that is, a gap is formed between the loose body / optical fiber preform 10 and the partition 5, the first chamber 11 and the second chamber 12 are connected, which does not mean that the first chamber 11 and the second chamber 12 cannot work at the same time. For example, when the first chamber 11 is undergoing a deposition process, the second chamber 12 can be sintered or even dehydrated by simply filling it with an inert gas, and the inert gas flowing from the second chamber 12 to the first chamber 11 will not affect the reaction atmosphere of the first chamber 11.
[0053] Therefore, in this embodiment, the first partition 51 and the third partition 53 between the first chamber 11 and the second chamber 12 can be made of rigid materials, and the partition between the second chamber 12 and the third chamber 13 can be made of flexible materials.
[0054] Before the deposition process, if the height difference between the lowest position of the target rod 4 and the first partition 51 is less than the total length of the loose body, then during the deposition process, as the target rod 4 is lifted, a situation as described above can be formed in which the loose body is simultaneously in the first chamber 11 and the second chamber 12, that is, the lower half of the loose body is in the first chamber 11, and the upper half is in the second chamber 12, so that the first chamber 11 and the second chamber 12 can simultaneously perform deposition treatment and dehydration treatment, or the first chamber 11 and the second chamber 12 can simultaneously perform deposition treatment and sintering treatment, so as to improve production efficiency.
[0055] If the first chamber 11 has a sufficient height so that the height difference between the lowest position where the target rod 4 sinks and the first partition 51 is greater than the total length of the loose body, the loose body can be deposited in the first chamber 11 and then lifted to the second chamber 12 for dehydration or sintering.
[0056] In one embodiment, the partition 5 is provided in the second chamber 12, and the partition 5 divides the second chamber 12 into a sintering chamber 121 and a dehydration chamber 122 which are connected up and down, and the sintering chamber 121 and the dehydration chamber 122 are respectively configured to perform the sintering process and the dehydration process on the loose body.
[0057] In one embodiment, a height of at least one of the sintering chamber 121 and the dehydration chamber 122 is smaller than a total length of the loose body, so that the sintering chamber 121 and the dehydration chamber 122 can perform the dehydration process and the sintering process simultaneously.
[0058] In one embodiment, the height of the second chamber 12 is smaller than the total length of the loose body, so that the first chamber 11, the sintering chamber 121 and the dehydration chamber 122 can simultaneously perform the deposition process, the dehydration process and the sintering process.
[0059] In one embodiment, the heights of the sintering chamber 121 and the dehydration chamber 122 are both greater than the total length of the loose body, so that the loose body can be dehydrated and sintered as a whole in the sintering chamber 121 and the dehydration chamber 122 respectively.
[0060] In one embodiment, the height of the third chamber 13 is greater than the total length of the optical fiber preform 10 , so that the optical fiber preform 10 can be annealed in the third chamber 13 as a whole.
[0061] In one embodiment, the partitions 5 are made of a rigid material, and a preset gap is provided between the through hole on each partition 5 and the loose body or the optical fiber preform 10 .
[0062] In one embodiment, the partition 5 is made of a flexible material, and the aperture of the through hole on each partition 5 is correspondingly smaller than the diameter of the loose body or the optical fiber preform 10, so that the partition 5 and the loose body or the optical fiber preform 10 are interference-fitted.
[0063] In one embodiment, the separator 5 is made of ceramic fiber.
[0064] In one embodiment, a third partition 53 is provided in the second chamber 12, and the third partition 53 divides the second chamber 12 into a sintering chamber 121 and a dehydration chamber 122 connected up and down. The sintering chamber 121 and the dehydration chamber 122 are respectively configured to sinter and dehydrate the loose body.
[0065] In one embodiment, the height of the sintering chamber 121 and / or the dehydration chamber 122 may be smaller than the total length of the loose body, so that the sintering chamber 121 and the dehydration chamber 122 can perform dehydration and sintering simultaneously, thereby improving production efficiency.
[0066] In one embodiment, the sum of the heights of the sintering chamber 121 and the dehydration chamber 122 may be less than the total length of the loose body, so that the first chamber 11, the sintering chamber 121 and the dehydration chamber 122 can simultaneously perform deposition, dehydration and sintering processes.
[0067] In one embodiment, the height of the third chamber 13 is greater than the total length of the optical fiber preform 10, so that the optical fiber preform 10 can be annealed as a whole in the third chamber 13, thereby ensuring that during annealing, stresses in multiple parts of the entire optical fiber preform 10 are reduced synchronously.
[0068] In one embodiment, the first chamber 11, the second chamber 12, and the third chamber 13, and even the sintering chamber 121 and the dehydration chamber 122 that constitute the second chamber 12, can be set to have a height greater than the total length of the loose body / optical fiber preform 10, so that deposition, dehydration, sintering, and annealing processes can be performed separately. The heights of the first chamber 11, the second chamber 12, and the third chamber 13 can be adaptively selected based on preparation requirements, and the above is only an exemplary description.
[0069] That is, the implementer can adaptively adjust the heights of the multiple chambers based on the process requirements of the optical fiber preform to be prepared, as well as the ratio of time consumed by deposition, dehydration, sintering and annealing processes, so as to make the preparation device suitable for uninterrupted preparation.
[0070] The preparation device and method are described below using examples.
[0071] Case
[0072] See also Figure 1In this case, the reaction chamber 1 includes a deposition chamber (first chamber 11), a dehydration chamber 122, a sintering chamber 121 (together with the dehydration chamber 122 to form the second chamber 12) and an annealing chamber (third chamber 13) arranged in sequence from bottom to top. The sum of the heights of the deposition chamber, the dehydration chamber 122 and the sintering chamber 121 is less than the total length of the optical fiber preform 10 to be prepared, and the height of the annealing chamber is greater than the total length of the optical fiber preform 10 to be prepared.
[0073] Based on the VAD method, the process of preparing the optical fiber preform by the preparation device is as follows:
[0074] The top of the target rod 4 is fixed to the chuck to ensure that the target rod 4 is in a vertical state. After the target rod 4 is moved into the reaction chamber 1, the reaction chamber 1 is sealed. The driving mechanism 3 drives the target rod 4 to move down to the bottom end of the target rod 4 and place it in the deposition chamber.
[0075] The control system 7 controls the feeding system to feed SiCl4 and other dopant materials to the core rod deposition lamp and the cladding deposition lamp according to the preset flow value. The core rod deposition lamp is first ignited to generate a powder with SiO2 as the main component, and sprayed on the target rod 4 to form a core rod. The cladding deposition lamp is then ignited to spray outside the core rod to form a cladding. At the same time, the control system 7 controls the driving mechanism 3 to drive the target rod 4 to rotate and lift, and prepares a loose body with a specific core-wrapping ratio and diameter that grows along the axial direction of the target rod 4.
[0076] During the preparation of the loose body, the position sensor and the online monitoring device continuously monitor the end position of the loose body, the running speed, the running distance, the diameter of the optical fiber preform 10, the transmittance of the optical fiber preform 10, the deposition feed amount, the hydrogen-oxygen flame gas flow rate of the blowtorch 6 and other information, which serve as the basis for the control system 7 to control the flame temperature of the blowtorch 6, the rotation and lifting speed of the driving mechanism 3, the feeding speed, the temperature of the deposition chamber and the gas atmosphere and other parameters.
[0077] As the target rod 4 is lifted, the loose body enters the dehydration chamber 122. When the control system 7 receives the sensing signal transmitted by the position sensor located in the dehydration chamber 122, the control system 7 controls the heating device in the dehydration chamber 122 to operate and heats the dehydration chamber 122 to 1300°C to dehydrate the loose body. After dehydration, the hydroxyl content of the core rod is less than or equal to 10ppb.
[0078] As the target rod 4 continues to rise, the loose body after dehydration enters the sintering chamber 121. When the control system 7 receives the sensing signal transmitted by the position sensor located in the sintering chamber 121, the control system 7 controls the heating device in the sintering chamber 121 to work, and heats the dehydration chamber 122 to 1500°C for sintering. During sintering, the gas distribution system introduces helium into the sintering chamber 121 to maintain a normal pressure of about 100Pa, and fluorine-containing gas can be introduced for fluorination treatment. Negative pressure sintering can be used when performing cladding sintering. At this time, no gas is passed and vacuum is performed to maintain negative pressure. The negative pressure is generally a vacuum below 0.01Pa, so as to eliminate the closed bubbles remaining in the optical fiber preform 10 after vitrification, improve the quality of the optical fiber preform and shorten the subsequent annealing time. An optical fiber preform 10 with a diameter of more than 90 mm, good core rod and cladding quality, and a minimum relative refractive index of -0.006 is sintered. The online monitoring device located in the sintering chamber 121 collects parameters such as the transmittance of the optical fiber preform 10 after sintering, so that the control system 7 controls the rotation and lifting speed of the driving mechanism 3 based on the above parameters, adjusts the deposition speed and the gas atmosphere in the deposition chamber, etc., to ensure the quality of the optical fiber preform 10.
[0079] As the target rod 4 is lifted, the sintered optical fiber preform 10 as a whole enters the annealing chamber for annealing treatment. In a high temperature environment, the gas distribution system introduces inert gases such as helium or nitrogen into the annealing chamber to reduce the internal stress of the optical fiber preform 10 and prevent the optical fiber preform 10 from cracking due to excessive stress. Finally, a large-size optical fiber preform 10 with a length of more than 2000 mm is prepared.
[0080] The obtained high-quality optical fiber preform 10 is moved out of the reaction chamber 1, and the optical fiber preform 10 is removed.
[0081] During the deposition process, the loose body lifted to the dehydration chamber 122 or even the sintering chamber 121 can be dehydrated or sintered simultaneously. Considering that the deposition process speed is slower than the dehydration and sintering processes, the dehydration and sintering processes can be performed intermittently.
[0082] The annealing treatment can be performed in an annealing chamber after the entire loose body is sintered to form the optical fiber preform 10, to ensure that the entire optical fiber preform 10 is annealed as a whole, so that the stress of multiple parts can be reduced synchronously, avoiding inconsistent stress elimination of multiple parts of the optical fiber preform 10.
[0083] Optionally, in addition to helium, the inert gas used as the reaction atmosphere may also be argon gas having good thermal conductivity.
[0084] This embodiment also provides a method for preparing an optical fiber preform using the above-mentioned preparation device, the method comprising:
[0085] The target rod 4 is placed in the first chamber 11, and a loose body is deposited on the target rod 4 by using a VAD method in the first chamber 11;
[0086] The target rod 4 is lifted, and the loose body in the second chamber 12 is dehydrated and sintered to obtain an optical fiber preform 10;
[0087] The optical fiber preform 10 is continuously lifted up, and the optical fiber preform 10 in the third chamber 13 is subjected to annealing treatment.
[0088] The implementation method of this method is basically the same as the above case and will not be described here in detail.
Claims
1. A device for preparing an optical fiber preform, comprising a reaction chamber (1), a holding mechanism (2) and a driving mechanism (3), wherein the holding mechanism (2) is arranged in the reaction chamber (1) and is arranged to fix a target rod (4), and the driving mechanism (3) is arranged to drive the holding mechanism (2) to rotate around a vertical axis and move up and down in a vertical direction, wherein: A plurality of partitions (5) are arranged in the reaction chamber (1), and the plurality of partitions (5) divide the reaction chamber (1) into a first chamber (11), a second chamber (12), and a third chamber (13) which are arranged in sequence from bottom to top; The partition (5) has a through hole, and the through hole is coaxially arranged with the target rod (4), so that the target rod (4) can be placed in the first chamber (11), the second chamber (12) or the third chamber (13) after moving in the vertical direction; The first chamber (11) is configured to deposit a loose body on the target rod (4) using an axial vapor deposition (VAD) method; The second chamber (12) is configured to perform a dehydration process and a sintering process on the loose body to obtain an optical fiber preform (10); The third chamber (13) is configured to perform annealing treatment on the optical fiber preform (10); The height of the third chamber (13) is greater than the total length of the optical fiber preform (10), so that the optical fiber preform (10) can be annealed as a whole in the third chamber (13).
2. The preparation device according to claim 1, wherein: The partition (5) is arranged in the second chamber (12), and the partition (5) divides the second chamber (12) into a sintering chamber (121) and a dehydration chamber (122) which are connected to each other up and down. The sintering chamber (121) and the dehydration chamber (122) are respectively configured to perform the sintering process and the dehydration process on the loose body.
3. The preparation device according to claim 2, wherein: The height of at least one of the sintering chamber (121) and the dehydration chamber (122) is smaller than the total length of the loose body, so that the sintering chamber (121) and the dehydration chamber (122) can perform the dehydration process and the sintering process simultaneously.
4. The preparation device according to claim 3, wherein: The height of the second chamber (12) is smaller than the total length of the loose body, so that the first chamber (11), the dehydration chamber (122) and the sintering chamber (121) can simultaneously perform deposition processing, the dehydration processing and the sintering processing.
5. The preparation device according to claim 2, wherein: The heights of the sintering chamber (121) and the dehydration chamber (122) are both greater than the total length of the loose body, so that the loose body can be dehydrated and sintered as a whole in the dehydration chamber (122) and the sintering chamber (121), respectively.
6. The preparation device according to any one of claims 1 to 5, wherein: The partitions (5) are made of a rigid material, and a preset gap is provided between the through hole on each of the partitions (5) and the loose body or the optical fiber preform (10).
7. The preparation device according to any one of claims 1 to 5, wherein: The partition (5) is made of a flexible material, and the diameter of the through hole on each of the partitions (5) is smaller than the diameter of the loose body or the optical fiber preform (10), so that the partition (5) and the loose body or the optical fiber preform (10) are interference-fitted.
8. The preparation device according to claim 7, wherein: The separator (5) is made of ceramic fiber.
9. The preparation device according to claim 1, wherein: The driving mechanism (3) comprises a first power assembly (31) and a second power assembly (32). The first power assembly (31) comprises a screw rod (311) extending from the top of the reaction chamber (1) into the third chamber (13) in a vertical direction, the lower end of the screw rod (311) being rotatably connected to a support member (312) fixedly connected to a chamber wall of the reaction chamber (1) corresponding to the third chamber (13), the upper end of the screw rod (311) being transmission-connected to a synchronous pulley mechanism (313), and the synchronous pulley mechanism (313) being driven by a first motor (314). The second power assembly (32) comprises a lifting seat (321) threadedly connected to the screw rod (311), and a second motor (322) fixed to the lifting seat (321).
10. The preparation device according to claim 1, further comprising: Control system (7), The control system (7) comprises a control module and an information acquisition module, wherein the control module comprises a programmable logic controller (PLC) and an operation console, and the information acquisition module comprises a position sensor and an online monitoring device arranged in at least one of the following: the first chamber (11), the second chamber (12), or the third chamber (13), The information acquisition module is configured to provide at least one of the following information to the control module: the acquired loose body end position, running speed, running distance, diameter of the optical fiber preform (10), transmittance of the optical fiber preform (10), deposition feed amount, and hydrogen-oxygen flame gas flow rate of the blowtorch (6); The control module is configured to adjust the start and stop and operating states of the heating device, feeding system, gas distribution system, blowtorch (6) and driving mechanism (3) in the optical fiber preform preparation device according to the information, so as to control the amount of loose body deposition and the temperature of the sintering chamber.
11. A method for preparing an optical fiber preform, applied to the optical fiber preform preparation device according to any one of claims 1 to 10, the method comprising: Placing the target rod (4) in the first chamber (11), and depositing a loose body on the target rod (4) in the first chamber (11) using an axial vapor deposition (VAD) method; The target rod (4) is lifted, and the loose body in the second chamber (12) is subjected to a dehydration treatment and a sintering treatment to obtain an optical fiber preform (10); The optical fiber preform (10) is continuously lifted, and an annealing treatment is performed on the optical fiber preform (10) in the third chamber (13).
Citation Information
Patent Citations
Equipment for loose body optical fiber prefabricated rod integral sintering desaeration and method thereof
CN101781087A
Device and method for manufacturing optical fiber preform
CN105502917A
Device and method for continuously preparing optical fiber preform rods and achieving drawing
CN108046582A
Total synthesis oversize ultra-low-water-peak optical fiber preform manufacturing equipment
CN202022852U
Prepare device of optical fiber perform and wire drawing in succession
CN207987041U