Preparation method and application of highly dispersed nano Co-Ni alloy catalyst

By uniformly dispersing Ni2+ and Co2+ in the catalyst using lignite ion exchange reaction, and preparing nanoCo-Ni alloy catalysts through pyrolysis and carbonization, the problems of large particle size, poor dispersion and ease of inactivation in the prior art are solved, and the problem of catalysts in the prior art is achieved. The stability and carbon deposit resistance in high temperature environments reduce the preparation cost and are suitable for industrial applications.

CN116237051BActive Publication Date: 2024-11-01CHINA UNIV OF MINING & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310283184.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-11-01
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

The existing Ni-Co bimetallic catalysts are prepared by impregnation, resulting in large metal particle size, poor dispersion, weak metal-support interactions, easy to sinter and decompose carbon deposits in high-temperature reactions, and limited precious metal resources, making it difficult to industrialize on a large scale. application.

Method used

Lignite is used as the carbon precursor, and Ni2+ and Co2+ are uniformly dispersed through ion exchange chemical reactions. After pyrolysis and carbonization, a highly dispersed nanoCo-Ni alloy catalyst is obtained to ensure that the metal particle size is small and the metal-support interaction is strong.

Benefits of technology

The prepared high-dispersible nano Co-Ni alloy catalyst is used stably in high temperature and high pressure environments, has good carbon deposits and sintering resistance, has a long service life and low cost, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116237051B_ABST
    Figure CN116237051B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a highly dispersed nano Co-Ni alloy catalyst, which belongs to the field of catalytic materials. Lignite is used as a carbon precursor, and its characteristics of being rich in carboxyl oxygen-containing functional groups are utilized to react with Ni in a mixed solution under alkaline conditions. 2+ and Co 2+ An ion exchange chemical reaction occurs, that is, the H + with Ni 2+ and Co 2+ Ion exchange occurs; due to the disordered distribution of carboxyl groups in the lignite structure, Ni 2+ and Co 2+ The catalyst is dispersed more evenly in the coal matrix. The coal precursor is then pyrolyzed and carbonized to remove volatiles to obtain a highly dispersed nano Co-Ni alloy catalyst. It is simple to prepare, has good use effect, can be used stably under high temperature and high pressure environment, is not prone to sintering and carbon deposition and deactivation, and has a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a highly dispersed nano Co-Ni alloy catalyst, belonging to the field of catalytic materials. Background Art

[0002] The introduction of metal co-acting Co on Ni-based catalysts to prepare Ni-Co bimetallic catalysts has a certain effect on improving the activity and stability of methane dry reforming reactions. However, the main method for introducing metal Co is the impregnation method. Although this method is convenient and fast, Co is mainly loaded onto the carrier by physical adsorption, resulting in a weak interaction between metal Co and the carrier, and the active components are easily lost in the actual reaction; the Ni-Co bimetallic catalyst prepared by the traditional impregnation method has large metal particle size, poor dispersibility, weak metal-carrier interaction, and is prone to carbon deposition and metal sintering in the pressurized low-temperature methane dry reforming reaction, resulting in rapid deactivation. The Co loaded by the impregnation method usually exists on the catalyst surface in the form of clusters, resulting in large metal particle size and poor dispersibility, and it is difficult to form an alloy with Ni, which is not conducive to better catalytic performance.

[0003] Literature reports (JH Bitter, J Catal. 1997, 171, 279-286) point out that precious metal catalysts have higher activity and anti-coking performance, but precious metal resources are limited, expensive, and difficult to apply on a large scale in industry. Ni-based catalysts have great potential for industrial application because of their high activity and low price. However, Ni-based catalysts are prone to sintering and carbon deposition during high-temperature reactions, resulting in rapid deactivation of the catalyst, which hinders the pace of its industrial application. Modification of Ni-based catalysts with precious metals is a common method, among which impregnation is the most commonly used method. In catalysts prepared by impregnation, precious metals are often wrapped by metal Ni, and precious metals exposed on the outer surface are less, precious metal utilization is low, and the activity and anti-coking performance of the catalyst need to be further improved. Summary of the invention

[0004] Technical problem: The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a highly dispersed nano Co-Ni alloy catalyst and its application, wherein metal Ni and Co are loaded onto a catalyst carrier through a chemical reaction, and the ratio between Ni and Co is adjusted to obtain a Ni-Co alloy catalyst with good dispersion, small metal particle size and strong metal-carrier interaction.

[0005] Technical solution: To achieve the above technical objectives, the present invention provides a method for preparing a highly dispersed nano Co-Ni alloy catalyst, using lignite as a carbon precursor, and utilizing its rich carboxyl oxygen-containing functional groups to react with Ni in a mixed solution under alkaline conditions. 2+ and Co 2+An ion exchange chemical reaction occurs, that is, the H + with Ni 2+ and Co 2+ Ion exchange occurs; due to the disordered distribution of carboxyl groups in the lignite structure, Ni 2+ and Co 2+ The catalyst is more evenly dispersed in the coal matrix; the coal precursor is then pyrolyzed and carbonized to remove volatiles to obtain a highly dispersed nano Co-Ni alloy catalyst.

[0006] The specific steps are as follows:

[0007] S1. Pre-treating lignite: acid washing and oxidation of lignite to ensure that the ash / dry basis content of the pre-treated lignite is 0.7wt%-9.2wt% and the carboxyl concentration is 1.83mmol / g-3.84mmol / g;

[0008] S2, preparing a mixed solution of cobalt acetate and nickel nitrate, wherein each liter of the mixed solution contains 0.15g-1.49g of cobalt acetate tetrahydrate, 0.18-1.75g ​​of nickel nitrate hexahydrate, and the rest is water; the purity of the cobalt acetate tetrahydrate is 99.5%, and the purity of the nickel nitrate hexahydrate is 98%;

[0009] S3. Add ammonium carbonate, ammonia water and pretreated lignite to the prepared mixed solution, and then stir: add 80 mL of ammonia water with an ammonia content of 25%-27%, 14.3 g of ammonium carbonate and 33.3 g of lignite per liter of the mixed solution. During the stirring process, the H + with Ni 2+ and Co 2+ Ion exchange occurs, Ni 2+ and Co 2+ will be more evenly dispersed into the coal matrix of lignite;

[0010] S4, filtering the stirred product to obtain a lignite precursor, adjusting the lignite precursor to neutrality by washing, and then drying the lignite precursor;

[0011] S4, placing the dried solid into an argon atmosphere tube furnace for carbonization pyrolysis, Ni 2+ and Co 2+ It is reduced to zero-valent metal to play an active role, and impurities in the lignite precursor are also removed in the process;

[0012] S5. After the pyrolysis is completed, the furnace temperature is lowered and the catalyst is taken out to obtain a highly dispersed nano Co-Ni alloy catalyst in which Ni, Co and the formed alloy are evenly distributed on the catalyst without metal agglomeration. The catalyst can be used stably under high temperature and high pressure environment and is not prone to sintering or carbon deposition and deactivation.

[0013] Furthermore, the lignite used has a particle size of 16-40 mesh.

[0014] Furthermore, the carbonization pyrolysis temperature was 650°C, wherein the heating rate of the tubular furnace was 10° / min, and the temperature was maintained at 650°C for 1 h.

[0015] A method for preparing a highly dispersed nano Co-Ni alloy catalyst is disclosed. The highly dispersed nano Co-Ni alloy catalyst is prepared.

[0016] The invention discloses an application of a highly dispersed nano Co-Ni alloy catalyst in preparing synthesis gas by dry reforming of methane. The temperature used for preparing synthesis gas by dry reforming of methane is 600-900°C and the pressure is 0.2-3.0MPa.

[0017] Beneficial effects: The highly dispersed nano Co-Ni alloy catalyst recorded in the present invention is cheap and has a relatively simple preparation process; the low-rank lignite used is abundant in my country and relatively cheap, and its use as a carbon precursor can reduce the catalyst preparation cost to a certain extent. Moreover, the Ni-Co / C bimetallic catalyst obtained after carbonization can be directly put into the methane dry reforming reaction without H2 activation. At the optimal Ni and Co mass ratio, the average particle size of the metal particles on the catalyst is only 4.85nm and exhibits good dispersibility; under the pressurized low temperature conditions of 0.3MPa and 650°C, the catalyst runs stably for 30h and exhibits good anti-coking and anti-sintering properties. After the reaction, the average particle size of the metal on the catalyst is only 5.84nm. The highly dispersed nano Co-Ni alloy catalyst recorded in the present invention can be stably used under high temperature and high pressure environments, and is not prone to sintering and carbon deposition and deactivation, and has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 TEM images and metal particle size distribution diagrams of the catalysts at three different Ni and Co concentration ratios in the embodiment of the present invention, specifically, TEM images and metal particle size distribution diagrams of three groups of Ni and Co at 0.05M and 0.1M, 0.075M and 0.075M, and 0.1M and 0.05M;

[0019] Figure 2 In the embodiment of the present invention, when Ni and Co are 0.05M and 0.1M, a is Ni 0.05 -Co 0.1a is the transmission electron microscope energy spectrum, b is the metal Ni energy spectrum scanning diagram, and c is the metal Co energy spectrum scanning diagram;

[0020] Figure 3 In the embodiment of the present invention, when Ni and Co are 0.05M and 0.1M, a is Ni 0.05 -Co 0.1 a is a high-resolution transmission electron microscope image, b is a diffraction pattern of the metal particle lattice;

[0021] Figure 4 The stability of three groups of catalysts with different Ni and Co configurations in the embodiment of the present invention was evaluated. The reaction conditions were: temperature, 650°C; pressure, 0.3MPa; CH4, CO2 molar ratio, 1:1; catalyst mass, 0.5g; CH / CO2 flow rate, 60mL / min;

[0022] Figure 5 In the embodiment of the present invention, Ni 0.05 -Co 0.1 Transmission electron microscopy image and metal particle size distribution after 30 hours of reaction. DETAILED DESCRIPTION

[0023] The present invention will be further described below with reference to the examples in the accompanying drawings:

[0024] A method for preparing a highly dispersed nano Co-Ni alloy catalyst, using lignite as a carbon precursor, utilizing its rich carboxyl oxygen-containing functional groups to react with Ni in a mixed solution under alkaline conditions 2+ and Co 2+ An ion exchange chemical reaction occurs, that is, the H + with Ni 2+ and Co 2+ Ion exchange occurs; due to the disordered distribution of carboxyl groups in the lignite structure, Ni 2+ and Co 2+ The obtained coal precursor is then pyrolyzed and carbonized to remove volatiles to obtain a highly dispersed nano Co-Ni alloy catalyst.

[0025] The specific steps are as follows:

[0026] S1. Pre-treating lignite: acid washing and oxidation of lignite to ensure that the ash / dry basis content of the pre-treated lignite is 0.7wt%-9.2wt%, and the carboxyl concentration is 1.83mmol / g-3.84mmol / g; the lignite particle size is 16-40 mesh;

[0027] S2, preparing a mixed solution of cobalt acetate and nickel nitrate, wherein each liter of the mixed solution contains 0.15g-1.49g of cobalt acetate tetrahydrate, 0.18-1.75g ​​of nickel nitrate hexahydrate, and the rest is water; the purity of the cobalt acetate tetrahydrate is 99.5%, and the purity of the nickel nitrate hexahydrate is 98%;

[0028] S3. Add ammonium carbonate, ammonia water and pretreated lignite to the prepared mixed solution, and then stir: add 80 mL of ammonia water with an ammonia content of 25%-27%, 14.3 g of ammonium carbonate and 33.3 g of lignite per liter of the mixed solution. During the stirring process, the H + with Ni 2+ and Co 2+ Ion exchange occurs, Ni 2+ and Co 2+ will be more evenly dispersed into the coal matrix of lignite;

[0029] S4, filtering the stirred product to obtain a lignite precursor, adjusting the lignite precursor to neutrality by washing, and then drying the lignite precursor;

[0030] S4, placing the dried solid into an argon atmosphere tube furnace for carbonization pyrolysis, Ni 2+ and Co 2+ It is reduced to zero-valent metal to play an active role, and impurities in the lignite precursor are also removed in this process; the carbonization pyrolysis temperature is 650℃, the heating rate of the tubular furnace is 10° / min, and it is maintained at 650℃ for 1h;

[0031] S5. After the pyrolysis is completed, the furnace temperature is lowered and the catalyst is taken out to obtain a highly dispersed nano Co-Ni alloy catalyst in which Ni, Co and the formed alloy are evenly distributed on the catalyst without metal agglomeration. The catalyst can be used stably under high temperature and high pressure environment and is not prone to sintering or carbon deposition and deactivation.

[0032] A method for preparing a highly dispersed nano Co-Ni alloy catalyst is disclosed. The highly dispersed nano Co-Ni alloy catalyst is prepared.

[0033] The invention discloses an application of a highly dispersed nano Co-Ni alloy catalyst in preparing synthesis gas by dry reforming of methane. The temperature used for preparing synthesis gas by dry reforming of methane is 600-900°C and the pressure is 0.2-3.0MPa.

[0034] Embodiment 1

[0035] Preparation of catalyst.

[0036] (1) First, three cups of 300 mL cobalt acetate and nickel nitrate solutions containing 0.05 M and 0.1 M, 0.075 M and 0.075 M, and 0.1 M and 0.05 M, respectively, were prepared, and then an equal amount (7.0 g) of ammonium carbonate was added to each of the three solutions, followed by 25 mL of ammonia water, and finally an equal amount (10 g) of lignite with a particle size of 16-40 mesh was added, and mechanical stirring was performed for an equal time (12 h);

[0037] (2) After the stirred sample is filtered, washed to neutrality and dried, it is placed in an argon atmosphere tubular furnace, and the carbonization pyrolysis temperature is set to 650°C to remove the volatile matter in the lignite precursor. The heating rate of the tubular furnace is 10° / min, and it is maintained at 650°C for 1 hour. After the carbonization is completed, argon is continuously passed until the furnace temperature naturally drops to room temperature, then the catalyst sample is taken out and stored in a glass sample bottle for later use. The catalyst yield in this process is 60%.

[0038] By configuring different concentrations of Ni 2+ and Co 2+ The solution finally obtained three types of Ni x Co y alloy catalyst, where x and y represent the concentrations of the two metal ions in the solution. The mass ratios of Ni and Co on the three catalysts were 1:6, 1:2 and 1:10, respectively, as measured by inductively coupled plasma mass spectrometry. Figure 1 As shown, transmission electron microscopy revealed that when the mass ratio of metal Ni to Co was 1:10, the minimum average particle size of the metal particles was 4.85 nm.

[0039] To you 0.05 -Co 0.1 Further analysis revealed that the metal Ni and Co were evenly distributed on the catalyst, and no metal clusters formed by particle agglomeration were observed. Figure 2 As shown in a, b, and c; high-resolution and lattice diffraction images are clearly shown, such as Figure 3 As shown in a and b in Figure 1, the (111) interplanar spacing is 0.20 nm, verifying the formation of Ni-Co alloy.

[0040] The three catalysts were put into methane dry reforming reaction respectively. Under the relatively harsh conditions of 0.3MPa and 650℃, Ni 0.05 -Co 0.1 The best stability was shown in the continuous operation of 30h, and the deactivation rate was only 0.3%. -1 ,like Figure 4 shown.

[0041] After 30h of reaction, Ni 0.05 -Co 0.1Transmission electron microscopy characterization revealed that the average metal particle size in its structure increased slightly to 5.84 nm. Figure 5 As shown, the catalyst still has good dispersibility, which shows its good anti-sintering performance, which is also an important reason for maintaining its catalytic stability.

[0042] Application of catalyst in pressurized methane dry reforming reaction.

[0043] The reaction was carried out in a stainless steel micro-fixed bed catalytic evaluation device, and the production of H2, CO, CH4 and CO2 was detected in real time by online gas phase. The catalyst dosage was 0.5g, and it could be put into use directly without H2 reduction. Before the reaction, the catalytic temperature was first set to 650℃, and the system pressure was charged to 0.3MPa using the raw gas (CH4 / CO2). After stabilization, the CH4 / CO2 (1:1) flow rate was set to 60mL / min, and the gas production was detected every 30min, and the CH4 and CO2 conversion rates and the H2 / CO molar ratio were calculated.

Claims

1. An application of a highly dispersed nano Co-Ni alloy catalyst, characterized in that: Lignite is used as a carbon precursor, and its rich carboxyl oxygen-containing functional groups are used to react with Ni in the mixed solution under alkaline conditions. 2+ and Co 2+ An ion exchange chemical reaction occurs, that is, the H + with Ni 2+ and Co 2+ Ion exchange occurs; due to the disordered distribution of carboxyl groups in the lignite structure, Ni 2+ and Co 2+ The catalyst is dispersed more evenly in the coal matrix; the coal precursor is then pyrolyzed and carbonized to remove volatiles to obtain a highly dispersed nano Co-Ni alloy catalyst; The specific steps are as follows: S1. Pre-treating lignite: acid washing and oxidation of lignite to ensure that the ash / dry basis content of the pre-treated lignite is 0.7wt%-9.2wt% and the carboxyl concentration is 1.83mmol / g-3.84mmol / g; S2. A mixed solution of cobalt acetate and nickel nitrate is prepared, wherein each liter of the mixed solution contains 0.15 g to 1.49 g of cobalt acetate tetrahydrate, 0.18 g to 1.75 g of nickel nitrate hexahydrate, and the remainder is water; the purity of the cobalt acetate tetrahydrate is 99.5%, and the purity of the nickel nitrate hexahydrate is 98%; S3. Add ammonium carbonate, ammonia water and pretreated lignite to the prepared mixed solution, and then stir: add 80 mL of ammonia water with an ammonia content of 25%-27%, 14.3 g of ammonium carbonate and 33.3 g of lignite per liter of mixed solution. During the stirring process, the H + with Ni 2+ and Co 2+ Ion exchange occurs, Ni 2+ and Co 2+ will be more evenly dispersed into the coal matrix of lignite; S4, filtering the stirred product to obtain a lignite precursor, adjusting the lignite precursor to neutrality by washing, and then drying the lignite precursor; S5. Place the dried solid into an argon atmosphere tube furnace for carbonization pyrolysis. 2+ and Co 2+ It is reduced to zero-valent metal to play an active role, and impurities in the lignite precursor are also removed in the process; S6. After the pyrolysis is completed, the furnace temperature is lowered and the catalyst is taken out to obtain a highly dispersed nano Co-Ni alloy catalyst in which Ni, Co and the formed alloy are evenly distributed on the catalyst without metal agglomeration. Using highly dispersed nano Co-Ni alloy catalyst to produce synthesis gas in methane dry reforming at a temperature of 600-900 o C, the pressure is 0.2-3.0 MPa, and the highly dispersed nano Co-Ni alloy catalyst can be directly put into methane dry reforming reaction without H2 activation.

2. The use of the highly dispersed nano Co-Ni alloy catalyst according to claim 1, characterized in that: The lignite particle size used was 16-40 mesh.

3. The use of the highly dispersed nano Co-Ni alloy catalyst according to claim 1, characterized in that: The carbonization pyrolysis temperature is 650 o C, where the heating rate of the tube furnace is 10 o / min, at 650 o C for 1 h.