A catalyst and its preparation method and application
By mixing yellow sandstone with sludge and performing roasting and activation treatments, a sludge carbon catalyst with high catalytic activity and stability is formed, which solves the problem of the loss of active components of the existing CWPO catalyst in high chloride wastewater and the treatment of coked sludge. difficult problem, achieving efficient organic pollutant degradation and catalyst stability.
Patent Information
- Application Number
- CN202310111695.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-08
AI Technical Summary
Existing CWPO catalysts suffer from serious loss of active components in high-chloride wastewater, low catalytic activity, and it is difficult to efficiently treat coked sludge.
Yellow sandstone is mixed with sludge, and after drying, roasting and activation treatments, a variety of iron phases and silicon-oxygen bridges are formed, which promotes the decomposition of hydrogen peroxide, improves catalytic activity, and increases the specific surface area and pore volume through oxalic acid activation.
Maintaining high catalytic activity and stability in high-chloride organic wastewater improves the degradation efficiency of organic pollutants and extends the service life of the catalyst.
Smart Images

Figure CN116237057B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of water treatment, and in particular to a catalyst and a preparation method and application thereof. Background Art
[0002] Coking wastewater is produced in the process of high-temperature coke production, gas purification and by-product recovery. Its chemical composition is complex and contains a large amount of phenolic substances, cyanide, sulfide, heterocyclic compounds and polycyclic aromatic hydrocarbons. Therefore, in order to control and reduce its adverse effects on the environment, a combined process of physical and chemical pretreatment, biological treatment, deep treatment and reuse treatment is usually used to treat coking wastewater. A large amount of sludge will be produced during the treatment process, and some of the difficult-to-degrade organic matter in the wastewater will be adsorbed by the sludge. Therefore, if the sludge generated during the treatment of coking wastewater is not properly disposed of, it will cause harm to the environment. The conversion of sludge into high-value-added sludge carbon by high-temperature pyrolysis is a promising way to solve the problem of sludge treatment and disposal. Pyrolysis can not only remove harmful pollutants in sludge, kill pathogens in sludge, but also recover resources and energy. After high temperature, the sludge not only forms conductive graphite carbon, but also forms oxygen-containing functional groups with redox activity, transition metals and their oxides. Sludge carbon can act as an electron donor, acceptor and medium, acting as an electron transfer medium to further improve the catalytic performance, catalytic activation of oxidants such as persulfate, hydrogen peroxide (H2O2) and ozone to generate sulfate radicals (SO4 - ·), hydroxyl radical (·OH), superoxide radical (·O2 - ) and singlet oxygen non-radicals ( 1 O2) etc.
[0003] Chloride ion is the main anion in high-salinity industrial wastewater. It can affect the types of free radicals generated in the catalytic wet hydrogen peroxide oxidation reaction (CWPO), reduce the activity of the catalyst, and thus affect the degradation of organic matter. In leather and dye manufacturing wastewater, high concentrations of NaCl (>50g / L) can often be detected, but its effect on the degradation process of organic matter has not been well explained. - The presence of chlorine can lead to catalyst deactivation, inhibit organic degradation, and produce toxic chlorinated byproducts. The development of chlorine-resistant CWPO catalysts is a technical bottleneck in this field.
[0004] Yellow sandstone mainly contains carbonate minerals, as well as rhodochrosite and yellow potassium ferrosite. It is formed under high iron sulfate concentration and high temperature of 80-90℃. After exposure to air, the surface is dark brown, and the inside is yellow sandstone. Some natural iron minerals such as hematite and goethite promote the catalytic wet hydrogen peroxide oxidation reaction (CWPO) due to their iron content. Yellow sandstone contains elements such as manganese and iron that can serve as active components in the catalyst, but the effect of using it directly as a catalyst is very poor. Therefore, it is necessary to utilize the important components of yellow sandstone such as manganese and iron through modification methods to prepare an efficient CWPO catalyst to promote the efficient treatment of difficult-to-degrade organic wastewater. Summary of the invention
[0005] In view of this, one purpose of the present application is to provide a method for preparing a catalyst, which solves the problem of additional loading of active components by introducing yellow sandstone, a natural iron-containing mineral, and mixing it with sludge. At the same time, the original iron element in the raw material combines with oxygen, carbon, aluminum and other elements during the roasting and carbonization process to form a variety of iron phases (ferroferric oxide, iron-aluminum spinel, zero-valent iron, etc.), which can promote the circulation between divalent iron and trivalent iron in the CWPO reaction, so that a high content of catalytically active components can be maintained in wastewater under chlorine-containing media, accelerate the decomposition of hydrogen peroxide to produce hydroxyl radicals, and promote the CWPO reaction rate; in addition, the rich silica in yellow sandstone can promote the hydrogen peroxide to combine with the silicon-oxygen bridge in the silica through hydrogen bonds, thereby accelerating the rapid transfer of hydrogen peroxide from the liquid phase to the catalyst surface and strengthening the CWPO reaction.
[0006] Another object of the present application is to provide a catalyst.
[0007] Another object of the present application is to provide an application of a catalyst.
[0008] To achieve the above object, the first embodiment of the present application provides a method for preparing a catalyst, comprising:
[0009] The yellow sandstone is mixed with the sludge, and after first drying, a first organic acid is added to prepare a granular mixture;
[0010] The granular mixture is allowed to stand, dried, and then calcined under an inert atmosphere to obtain a crude catalyst product;
[0011] The crude catalyst product is impregnated and activated, and then impurities are removed and a second drying is performed to obtain the catalyst product.
[0012] In some embodiments, the yellow sandstone is yellow sandstone containing 3-5 wt % of jarosite mineral.
[0013] In some embodiments, the yellow sandstone is ground and sieved before being mixed with the sludge.
[0014] In some embodiments, the sludge is one or more of coking wastewater sludge, petrochemical wastewater sludge, and pharmaceutical wastewater sludge.
[0015] In some embodiments, the first organic acid is one or more of oxalic acid, acetic acid, and formic acid.
[0016] In some embodiments, the mass ratio of the yellow sandstone to the sludge is (1:10)-(1:8).
[0017] In some embodiments, the mass concentration of the first organic acid is 4-6%, and the added amount of the first organic acid is 0.3-0.6% of the total mass of the yellow sandstone and the sludge after the first drying.
[0018] In some embodiments, the coking sludge is sludge with a moisture content of 75-80% discharged from the reclaimed water treatment process in a coking wastewater treatment plant.
[0019] In some embodiments, the first drying includes natural air drying and / or oven drying.
[0020] In some embodiments, the standing temperature is room temperature, the standing time is 3-5 days, the drying temperature is 150-170° C., and the drying time is 12-24 hours.
[0021] In some embodiments, the natural air drying time is 5-7 days.
[0022] In some embodiments, the oven drying temperature is 105-120° C., and the oven drying time is 24-36 hours.
[0023] In some embodiments, the calcining is performed in an oxygen-free environment.
[0024] In some embodiments, the calcination temperature is 600-800° C., and the calcination time is 2-3 hours.
[0025] In some embodiments, the roasting is carried out in a carbonization converter, and the rotation speed of the carbonization converter during the roasting process is 3-8 r / min.
[0026] In some embodiments, the flow rate of the inert atmosphere during the calcination process is 200-300 mL / min.
[0027] In some embodiments, the impregnation liquid for impregnation activation is a second organic acid, and the second organic acid is one or more of oxalic acid, acetic acid, and formic acid.
[0028] In some embodiments, the impregnation activation is performed under sealed conditions, the temperature of the impregnation activation is room temperature, and the time of the impregnation activation is 10-15 hours.
[0029] In some embodiments, the impurity removal method is to rinse with ultrapure water until the eluent is neutral.
[0030] In some embodiments, the drying temperature of the second drying is 105-120° C., and the drying time of the second drying is 24-36 hours.
[0031] In order to achieve the above-mentioned purpose, a second embodiment of the present application proposes a catalyst, which is prepared using the catalyst preparation method of the embodiment of the present application.
[0032] To achieve the above-mentioned purpose, the third aspect of the embodiment of the present application relates to the application of the catalyst of the embodiment of the present application in water treatment.
[0033] The catalyst of the embodiment of the present application can bring the following beneficial effects:
[0034] 1. This application solves the problem of additional loading of active components by introducing yellow sandstone, a natural iron-containing mineral, and mixing it with iron-containing sludge. The original iron element in the raw material combines with oxygen, carbon, aluminum and other elements during the roasting and carbonization process to form a variety of iron phases (ferroferric oxide, iron-aluminum spinel, zero-valent iron, etc.), which promotes the circulation between divalent iron and trivalent iron in the CWPO reaction, thereby maintaining a high content of catalytic active components in wastewater under chlorine-containing media, accelerating the decomposition of hydrogen peroxide to produce hydroxyl radicals, and promoting the CWPO reaction.
[0035] 2. The present application performs high-temperature roasting and carbonization on the sludge, which can fix the heavy metals and carbon elements in the sludge. At the same time, the sludge used in the present application can be selected from the coking sludge in the reclaimed water treatment link of the coking wastewater treatment plant in a certain industrial park. Since an iron-containing coagulant is added to the reclaimed water treatment link, the iron content in the coking sludge produced is rich (up to 28.32wt%), which can be effectively converted into the active component of the CWPO catalyst without the need for additional loading of active components, thereby reducing the preparation cost of the catalyst. In addition, during the roasting and carbonization process, the iron and carbon structures are tightly combined and are not easy to lose, and can maintain a high catalytic activity and stability in the treatment of high-chloride organic wastewater.
[0036] 3. Yellow sandstone is a natural green environmentally friendly material, which is widely used in public buildings, villas and indoor and outdoor decoration. It has the advantages of no pollution and no radioactivity. The flexural strength of yellow sandstone is stronger than that of granite, and its compressive strength and wear resistance are between granite and marble. It has low water absorption and good acid resistance. Therefore, the sludge carbon catalyst prepared by mixing yellow sandstone into sludge in a certain proportion has good strength, is used to treat organic wastewater, has good resistance to hydraulic shock, and has good catalytic stability in acidic environment. At the same time, the yellow potassium iron alum in yellow sandstone can increase the catalytic active sites of hydrogen peroxide, promote its decomposition to produce hydroxyl free radicals, thereby improving the catalytic degradation efficiency of organic pollutants. In addition, the rich silicon dioxide in yellow sandstone can promote the hydrogen peroxide to combine with the silicon oxygen bridge in silicon dioxide through hydrogen bonding, thereby accelerating the rapid transfer of hydrogen peroxide from the liquid phase to the surface of the sludge carbon catalyst and strengthening the CWPO reaction.
[0037] 4. The use of organic acids such as oxalic acid as activators in this application has the following advantages:
[0038] ① It can promote the formation of various oxygen-containing functional groups on the surface of yellow sandstone modified sludge carbon, which is beneficial to combine with difficult-to-degrade organic matter containing hydroxyl structure through hydrogen bonding and with difficult-to-degrade organic matter containing benzene ring structure through π-π action, thereby promoting its free radical oxidation degradation on the catalyst surface.
[0039] ② The activation energy of organic acids such as oxalic acid can effectively increase the specific surface area and pore volume of the yellow sandstone modified sludge carbon catalyst.
[0040] ③ Organic acids such as oxalic acid are medium-strong acids that can maintain the strength of sludge charcoal, dissolve less ash in the sludge charcoal, preserve the content of active components to a great extent, and increase the physical phases of iron in different valence states, thereby improving the activity and service life of the catalyst and facilitating its recycling and reuse.
[0041] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0043] Figure 1 is a scanning electron microscope (SEM) comparison diagram of the catalyst YCC-M (1) of Example 1, wherein:
[0044] (a) is a scanning electron microscope (SEM) image with a scale bar of 100 μm and a magnification of 200 times;
[0045] (b) is a scanning electron microscope (SEM) image with a scale bar of 10 μm and a magnification of 1000 times.
[0046] Figure 2 1 is a transmission electron microscope (TEM) comparison diagram of catalyst YCC-M (1) of Example 1, wherein:
[0047] (d) is a transmission electron microscope (TEM) image with a scale bar of 30 μm and a magnification of 5000 times;
[0048] (e) is a transmission electron microscope (TEM) image with a scale bar of 100 nm and a magnification of 5000 times;
[0049] (f) is a transmission electron microscopy (TEM) image with a scale bar of 50 nm and a magnification of 5000 times.
[0050] Figure 3 This is a particle size distribution diagram of catalyst YCC-M(1) of Example 1. DETAILED DESCRIPTION
[0051] The embodiments of the present application are described in detail below. The embodiments are exemplary and intended to be used to explain the present application, but should not be construed as limiting the present application.
[0052] Throughout the application, the disclosure of numerical ranges includes all values within the entire range and disclosure of further subdivided ranges, including endpoints and subranges given within those ranges.
[0053] In the application, the raw materials, equipment, etc. involved, unless otherwise specified, are all raw materials and equipment that can be produced through commercial channels or known methods; the methods involved, unless otherwise specified, are all conventional methods.
[0054] The inventors found that, on the one hand, most of the CWPO catalysts currently available on the market are supported catalysts, that is, certain catalytically active components such as iron, manganese and other elements are loaded on catalyst carriers such as zeolite, molecular sieves, metal oxides and biochar. However, this type of supported catalyst often has a serious problem of active component loss after use. In addition, this type of catalyst has poor catalytic activity in high-chloride wastewater, because the corrosion of chloride ions on the catalyst causes its active components to lose faster. Coking wastewater is a high-concentration, highly polluted organic wastewater with high toxicity and poor biodegradability. It is the most difficult type of wastewater to treat in the steel industry. At present, pretreatment + biochemical treatment + coagulation sedimentation treatment process is generally adopted. A large amount of sludge will be produced in the biochemical and coagulation treatment stages. This part of the sludge contains high concentrations of organic matter and pathogenic microorganisms. The "National List of Hazardous Wastes" (2016) stipulates that solid waste containing such components is hazardous waste. On the other hand, yellow sandstone is a natural green environmentally friendly material, widely used in public buildings, villas and indoor and outdoor decoration, with the advantages of no pollution and no radioactivity. The flexural strength of yellow sandstone is stronger than that of granite, and its compressive strength and wear resistance are between those of granite and marble. It also has low water absorption and good acid resistance. The potassium ferroaluminate in yellow sandstone can increase the catalytic active sites of hydrogen peroxide, promote its decomposition to produce hydroxyl radicals, and thus improve the catalytic degradation efficiency of organic pollutants. The abundant silica in yellow sandstone can promote the hydrogen peroxide to combine with the silicon-oxygen bridge in silica through hydrogen bonds, thereby accelerating the rapid transfer of hydrogen peroxide from the liquid phase to the surface of the sludge catalyst and strengthening the CWPO reaction.
[0055] The preparation method of the catalyst in the embodiment of the present application, its inventive concept is: in order to address the problems of serious loss of active components, low catalytic activity and difficult treatment of sludge such as coking sludge in high-chloride organic wastewater of sludge carbon catalyst, by carbonizing yellow sandstone containing potassium ferroaluminate, silicon dioxide, etc. mixed with coking sludge and other sludge to prepare a new sludge carbon catalyst, and then activating it with organic acids such as oxalic acid, finally obtaining a sludge carbon catalyst with high catalytic performance and stability in high-chloride organic wastewater.
[0056] The method for preparing the catalyst of the embodiment of the present application comprises the following steps:
[0057] S101, mixing yellow sandstone and sludge, and after a first drying, adding a first organic acid to prepare a granular mixture.
[0058] In some embodiments, the yellow sandstone contains 3-5 wt% jarosite minerals, which can enhance the catalytic activity of the sludge carbon and promote the rapid reaction of CWPO.
[0059] In some embodiments, the yellow sandstone needs to be ground and sieved before mixing with the sludge to ensure a smaller particle size and a larger specific surface area. Preferably, the grinding and sieving includes but is not limited to a 70-90 mesh sieve, such as an 80 mesh sieve.
[0060] In some embodiments, the sludge may be a sludge containing metal elements, including but not limited to one or more of iron-containing sludge, manganese-containing sludge, etc. As a non-limiting example, the sludge includes but is not limited to one or more of coking wastewater sludge, petrochemical wastewater sludge, pharmaceutical wastewater sludge, etc. It should be noted that the content of metal elements in the sludge in this application is not limited, as long as it is present, but the higher the content of metal elements, the more obvious the effect on improving the catalytic activity of the catalyst. As a non-limiting example, the content of metal elements in the sludge is between 2-15wt%. Preferably, the sludge is coking sludge, and specifically, the sludge with a water content of 75-80% discharged from the reclaimed water treatment link in the coking wastewater treatment plant can be selected. Since an iron-containing coagulant is added to the reclaimed water treatment link, the iron content in the coking sludge produced is rich (up to 28.32wt.%), which can be effectively converted into the active component of the CWPO catalyst, without the need for additional loading of active components, and the preparation cost of the catalyst can be reduced. In addition, during the subsequent roasting and carbonization process, the iron and carbon structures are tightly combined and are not easily lost, and can maintain high catalytic activity and stability in the treatment of high-chloride organic wastewater.
[0061] In some embodiments, the mass ratio of yellow sandstone to sludge is (1:10)-(1:8). As a non-limiting example, the mass ratio of yellow sandstone to sludge includes but is not limited to 1:10, 1:9.5, 1:9 or 1:8. When the mass ratio of yellow sandstone to sludge is within the above range, the catalyst activity is good; when it is less than 1:10, the catalyst activity becomes poor; when it is greater than 1:8, the catalyst activity also becomes poor.
[0062] In some embodiments, the first drying may be natural air drying only; in other embodiments, the first drying may be oven drying only; in yet other embodiments, the first drying may include both natural air drying and oven drying. Among them, natural air drying takes a long time, and oven drying takes a short time, but the energy consumption is relatively high. Therefore, in order to balance the time consumption and energy consumption, as a possible example, the first drying may be natural air drying first, and then oven drying. In some embodiments, the natural air drying time is 5-7d, including but not limited to 5d, 5.5d, 6d, 6.5d or 7d, etc.; the oven drying temperature is 105-120℃, including but not limited to 105℃, 110℃, 115℃ or 120℃, etc.; the oven drying time is 24-36h, including but not limited to 24h, 28h, 30h, 34h or 36h, etc.
[0063] In some embodiments, the first organic acid includes but is not limited to one or more of oxalic acid, acetic acid, and formic acid. In step S101, the purpose of adding the first organic acid such as oxalic acid is to activate the active components in the mixed sample of yellow sandstone and sludge.
[0064] In some embodiments, the mass concentration of the first organic acid is 4-6%, and the amount of the first organic acid added is 0.3-0.6% of the total mass of the yellow sandstone and the sludge after the first drying. As a non-limiting example, the mass concentration of the first organic acid is 4%, 4.5%, 5%, 5.5% or 6%, etc.; the amount of the first organic acid added is 0.3%, 0.4%, 0.5% or 0.6% of the total mass of the yellow sandstone and the sludge after the first drying. The mass concentration of the first organic acid is selected in the above range, and the obtained catalyst activity is higher; less than 4%, the activity is poor; greater than 6%, the activity is poor.
[0065] In some embodiments, the particles of the granular mixture include but are not limited to regular shapes such as spheres and cylinders, and irregular shapes such as special shapes. The preparation of the granular mixture includes but is not limited to using a molding device to prepare a granular mixture from a mixture of the first dried yellow sandstone, sludge and the first organic acid, wherein the molding device includes but is not limited to a catalyst spherical molding device, and the obtained granular mixture can be a uniform spherical mixture, for example, a uniform spherical mixture with a diameter of 1.5-3 mm.
[0066] S102, allowing the granular mixture to stand, drying, and then calcining under the protection of an inert atmosphere to obtain a crude catalyst product.
[0067] In some embodiments, the granular mixture is placed at room temperature for 3-5 days. By placing the mixture at rest, the yellow rock sand and the sludge can be more firmly combined. As a non-limiting example, the resting time includes but is not limited to 3 days, 3.5 days, 4 days, 4.5 days or 5 days.
[0068] In some embodiments, the drying temperature is 150-170° C., and the drying time is 12-24 hours. As non-limiting examples, the drying temperature includes but is not limited to 150° C., 155° C., 160° C., 165° C., or 170° C., and the drying time includes but is not limited to 12 hours, 15 hours, 18 hours, 21 hours, or 24 hours, etc.
[0069] In some embodiments, the roasting is carried out in a carbonization converter, and the speed of the carbonization converter during the roasting process is 3-8 r / min. As a non-limiting example, the speed of the carbonization converter during the roasting process includes but is not limited to 3 r / min, 4 r / min, 5 r / min, 6 r / min, 7 r / min or 8 r / min, etc.
[0070] In some embodiments, firing is performed in an oxygen-free environment.
[0071] In some embodiments, the inert atmosphere includes, but is not limited to, one or more of nitrogen, helium, or argon. The flow rate of the inert atmosphere is 200-300 mL / min. As a non-limiting example, the flow rate of the inert atmosphere includes, but is not limited to, 200 mL / min, 230 mL / min, 250 mL / min, 280 mL / min, or 300 mL / min, etc.
[0072] In some embodiments, the calcination temperature is 600-800° C., and the calcination time is 2-3 hours. As non-limiting examples, the calcination temperature includes but is not limited to 600° C., 650° C., 700° C., 750° C., or 800° C., and the calcination time includes but is not limited to 2 hours, 2.5 hours, or 3 hours.
[0073] As a possible example, the method for obtaining a crude catalyst product is: leaving the granular mixture at room temperature for a period of time, and then putting it into an oven for drying; before roasting in a carbonization converter, the air must be evacuated and filled with inert gases such as nitrogen, and then the roasting and carbonization process is carried out. After carbonization, it is naturally cooled to room temperature to obtain a crude catalyst product.
[0074] In the present application, the sludge is subjected to high temperature calcination and carbonization to fix the heavy metals and carbon elements in the sludge.
[0075] S103, impregnating and activating the crude catalyst product, and then removing impurities and performing a second drying to obtain a catalyst product.
[0076] In some embodiments, the impregnation liquid for impregnation activation is a second organic acid, and the second organic acid includes but is not limited to one or more of oxalic acid, acetic acid, and formic acid. Selecting an organic acid as an activator has the following advantages: ① It can promote the formation of a variety of oxygen-containing functional groups on the surface of yellow sandstone modified sludge carbon, which is beneficial to the combination with the difficult-to-degrade organic matter containing a hydroxyl structure through hydrogen bonding, and the combination with the difficult-to-degrade organic matter containing a benzene ring structure through π-π action, thereby promoting its free radical oxidation degradation on the catalyst surface. ② The activation energy of organic acids such as oxalic acid can effectively increase the specific surface area, pore volume, etc. of the yellow sandstone modified sludge carbon catalyst. ③ Organic acids such as oxalic acid are medium-strong acids that can maintain the strength of sludge carbon, have a small dissolution of ash in sludge carbon, preserve the content of active components to a great extent, and increase the physical phases of iron in different valence states, thereby improving the activity and service life of the catalyst, which is conducive to recycling and reuse.
[0077] In some embodiments, the mass concentration of the impregnation liquid for impregnation activation is 4-6%, that is, the mass concentration of the second organic acid such as one or more of oxalic acid, acetic acid, formic acid is 4-6%. As a non-limiting example, the mass concentration of the impregnation liquid for impregnation activation is 4%, 4.5%, 5%, 5.5% or 6%, etc.
[0078] In some embodiments, the impregnation activation is performed under sealed conditions, the impregnation activation temperature is room temperature, and the impregnation activation time is 10-15 hours. As a non-limiting example, the impregnation activation time includes but is not limited to 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, or 15 hours.
[0079] In some embodiments, the method for removing impurities is to rinse with ultrapure water until the eluent is neutral.
[0080] In some embodiments, the drying temperature of the second drying is 105-120° C., and the drying time of the second drying is 24-36 hours. As a non-limiting example, the drying temperature of the second drying includes but is not limited to 105° C., 110° C., 115° C., or 120° C., and the drying time of the second drying includes but is not limited to 24 hours, 28 hours, 30 hours, 34 hours, or 36 hours, etc.
[0081] The preparation method of the catalyst of the embodiment of the present application solves the problem of additional loading of active components by introducing yellow sandstone, a natural iron-containing mineral, and mixing it with iron-containing sludge. At the same time, the original iron element in the raw material combines with oxygen, carbon, aluminum and other elements during the roasting and carbonization process to form a variety of iron phases (ferroferric oxide, iron-aluminum spinel, zero-valent iron, etc.), which can promote the circulation between divalent iron and trivalent iron in the CWPO reaction, so that a high content of catalytically active components can be maintained in wastewater under chlorine-containing media, accelerate the decomposition of hydrogen peroxide to produce hydroxyl radicals, and promote the CWPO reaction rate; in addition, the abundant silicon dioxide in yellow sandstone can promote the combination of hydrogen peroxide and silicon-oxygen bridges in silicon dioxide through hydrogen bonds, thereby accelerating the rapid transfer of hydrogen peroxide from the liquid phase to the catalyst surface, and strengthening the CWPO reaction.
[0082] It should be noted that the "first" and "second" in "first organic acid", "second organic acid", "first drying", "second drying" etc. in the present application are only for distinction and convenience of expression and have no special meaning.
[0083] The catalyst of the embodiment of the present application is prepared by the preparation method of the catalyst of the embodiment of the present application.
[0084] The catalyst of the embodiment of the present application can be used for water treatment, including but not limited to high-chloride organic wastewater, pharmaceutical wastewater, chemical wastewater, etc.
[0085] As a possible example, high-chloride organic wastewater is the wastewater from the actual coking wastewater biochemical secondary effluent section of an industrial park. The wastewater is light yellow, has a pungent odor, a pH of 7.5-8.5, a COD of 200-300 mg / L, a TOC of 100-120 mg / L, and NH4 +-N is 15-25 mg / L, and the mass concentration of chloride ions is 3-5%. The wastewater is subjected to CWPO advanced oxidation treatment using the catalyst of the embodiment of the present application, and the reaction conditions are: temperature 25-35°C, pH 4-9, hydrogen peroxide 0.3-0.7 kg / t, and reactor space velocity 0.8-1.2 h -1 .
[0086] The catalysts and applications of the embodiments of the present application have the beneficial effects of the methods for preparing the catalysts of the embodiments of the present application.
[0087] Certain features of the present technology are further illustrated in the following non-limiting examples.
[0088] Example 1
[0089] The catalyst of this embodiment, its preparation method comprises the following steps:
[0090] (1) Grinding yellow sandstone containing 4 wt% jarosite through an 80-mesh sieve;
[0091] (2) Select coking sludge with a moisture content of 78% (iron content of 28.32 wt%) discharged from the reclaimed water treatment stage of a coking wastewater treatment plant, and mix the yellow sandstone ground in step (1) into the coking sludge, wherein the mass ratio of yellow sandstone to coking sludge is 1:10, and then naturally air-dry for 5 days, and then dry in an oven at 120°C for 24 hours.
[0092] (3) adding oxalic acid solution with a mass concentration of 4% to the product obtained in step (2) for mixing, wherein the amount of oxalic acid solution added is 0.3% of the mass of the dried yellow sandstone and coking sludge mixture, and then forming the mixture into uniform spheres using a catalyst spherical molding device to obtain a spherical mixture with a diameter of 2 mm;
[0093] (4) The spherical mixture in step (3) is placed at room temperature for 3 days, and then placed in an oven at a temperature of 150°C for drying for 24 hours, and then transferred to a carbonization converter for calcination. Before calcination, the air is first evacuated, and then nitrogen is introduced at a flow rate of 200 mL / min. The temperature is then raised to 600°C and maintained for 3 hours. The speed of the carbonization converter during calcination is 5 r / min. After calcination and carbonization, it is naturally cooled to room temperature to obtain a crude catalyst product (i.e., sludge charcoal).
[0094] (5) At room temperature and sealed conditions, the crude catalyst product obtained in step (4) was immersed in a 4% mass concentration oxalic acid solution for activation treatment for 10 hours; then rinsed with ultrapure water until the eluent was neutral, placed in an oven at 120° C. for 24 hours, and cooled to obtain the catalyst YCC-M (1) of this example.
[0095] Figure 1This is a scanning electron microscope (SEM) comparison image of the catalyst YCC-M (1) of Example 1. Figure 1 It can be seen that the prepared sludge carbon catalyst is a nano-sheet material, which is a material shape with high catalytic activity.
[0096] Figure 2 This is a transmission electron microscope (TEM) comparison diagram of catalyst YCC-M (1) of Example 1. Figure 2 It can be seen that the synthesized material is a typical carbon-based catalyst material with metal oxides loaded on the surface.
[0097] Figure 3 is a particle size distribution diagram of the catalyst YCC-M(1) of Example 1. Figure 3 It can be seen that the catalyst particles are uniform in size, with a particle size of about 25 microns.
[0098] application:
[0099] The wastewater from the biochemical secondary effluent section of a coking wastewater in an industrial park was taken as the treatment object (i.e., raw water). The wastewater was light yellow, had a pungent odor, a pH of 8.0, a COD of 223 mg / L, a TOC of 111 mg / L, and NH4 + -N is 23 mg / L, and the mass concentration of chloride ions is 4%. The catalyst YCC-M (1) of this example is used to carry out CWPO advanced oxidation treatment on the wastewater. The reaction conditions are: temperature 30°C, pH 7, hydrogen peroxide 0.5 kg / t (30 wt.%) and reactor space velocity 1 h -1 A control experiment 1 was set up, that is, no catalyst was added in the CWPO reaction stage, and other reaction conditions were the same; at the same time, the existing commercial catalyst Fe(II)@ZSM-5 was used instead of the catalyst of this example to carry out CWPO advanced oxidation treatment, and other reaction conditions were the same. The inlet and outlet water quality analysis and testing items involved chemical oxygen demand (COD), total organic carbon (TOC), ammonia nitrogen (NH4 + -N) etc. After adding the catalyst of this example, the CWPO treatment device (which is a conventional reaction device of CWPO, the specific structure is not repeated here) is allowed to run stably for a period of time until the effluent quality is stable, and the result is recorded in Table 1.
[0100] Table 1 Wastewater treatment effects of the catalyst of Example 1, control experiment 1, and commercial catalyst Fe(II)@ZSM-5
[0101]
[0102]
[0103] It can be seen from Table 1 that when treating coking wastewater of the same water quality and when the reaction condition pH is 7, the effluent water quality of the catalyst YCC-M (1) of this embodiment is significantly improved, especially the chemical oxygen demand (COD) removal rate is significantly improved, compared with the case where no catalyst is added or the catalyst is commercial Fe (II) @ ZSM-5.
[0104] Example 2
[0105] This embodiment is basically the same as Embodiment 1, except that:
[0106] During the application process, when the wastewater was subjected to CWPO advanced oxidation treatment, the pH value in the reaction conditions was 5; the case where the wastewater was treated without adding a catalyst was control experiment 2.
[0107] At the same time, for the convenience of description, in order to distinguish it from the catalyst in Example 1, the catalyst of this example is marked as catalyst YCC-M(2).
[0108] When the catalyst of this example, control experiment 2 without adding a catalyst, and the commercial catalyst Fe(II)@ZSM-5 were used for treatment, the treatment results are shown in Table 2.
[0109] Table 2 Wastewater treatment effects of the catalyst of Example 2, control experiment 2, and commercial catalyst Fe(II)@ZSM-5
[0110]
[0111] It can be seen from Table 2 that when treating coking wastewater of the same water quality and when the reaction condition pH is 5, the catalyst YCC-M(2) of this embodiment (essentially the catalyst of Example 1) has significantly improved effluent water quality compared to the case where no catalyst is added or the catalyst is commercial Fe(II)@ZSM-5, wherein the removal rates of chemical oxygen demand (COD) and total organic carbon (TOC) are comparable. At the same time, by comparing Table 1 and Table 2, it can be seen that when using the same catalyst of this application (the catalysts of Examples 1 and 2 are essentially the same), when treating coking wastewater of the same water quality and the reaction condition pH is 7, the removal rates of COD, TOC, and NH4 + -N removal rates were approximately 54.7%, 49.5% and 52.2% respectively. When the reaction condition was pH 5, the removal rates of COD, TOC, NH4 + The removal rates of -N were approximately 58.3%, 53.2% and 26.1%, respectively, indicating that the removal rate of organic matter was higher when the pH was lower, and the removal rate of NH4 + -N removal rate is high. The degradation efficiency of organic matter and ammonia nitrogen by the YCC-M catalyst prepared in this application is higher than that of the commercial Fe(II)@ZSM-5 catalyst and the control experimental group.
[0112] Example 3
[0113] This embodiment is basically the same as Embodiment 2, except that:
[0114] The wastewater quality indicators during the application process are different, specifically: pH is 5, COD is 260mg / L, TOC is 118mg / L, NH4 + -N is 25 mg / L, and the mass concentration of chloride ions is 5%.
[0115] The case where the wastewater was treated without adding a catalyst is referred to as control experiment 3.
[0116] At the same time, for the convenience of description, in order to distinguish it from the catalyst in Example 2, the catalyst of this example is marked as catalyst YCC-M(3).
[0117] When the catalyst of this example, control experiment 3 without adding a catalyst, and the commercial catalyst Fe(II)@ZSM-5 were used for treatment, the treatment results are shown in Table 3.
[0118] Table 3 Wastewater treatment effects of the catalyst of Example 3, control experiment 3, and commercial catalyst Fe(II)@ZSM-5
[0119]
[0120] It can be seen from Table 3 that when treating coking wastewater with higher water quality indexes and when the reaction condition pH is 5, the effluent water quality is still significantly improved by using the catalyst of this embodiment (substantially the catalyst of Example 1 and Example 2) compared with the case where no catalyst is added or the catalyst is commercial Fe(II)@ZSM-5. At the same time, by comparing Table 2 and Table 3, it can be seen that when the same catalyst of this application is used, when the reaction condition pH is 5 and other conditions remain unchanged, the COD, TOC, and NH4 + The removal rates of -N were stably higher than 58%, 52% and 24%, and were higher than those of the commercial Fe(II)@ZSM-5 catalyst and the control experimental group.
[0121] Example 4
[0122] The catalyst of this embodiment, its preparation method comprises the following steps:
[0123] (1) Grinding yellow sandstone containing 4 wt% jarosite through an 80-mesh sieve;
[0124] (2) Select coking sludge with a moisture content of 80% (iron content of 28.32 wt%) discharged from the reclaimed water treatment stage of a coking wastewater treatment plant, and mix the yellow sandstone ground in step (1) into the coking sludge, wherein the mass ratio of yellow sandstone to coking sludge is 1:8, then naturally air-dry for 7 days, and then dry in an oven at 110°C for 28 hours.
[0125] (3) adding oxalic acid solution with a mass concentration of 5% to the product obtained in step (2) and mixing them, wherein the amount of oxalic acid solution added is 0.5% of the mass of the dried yellow sandstone and coking sludge mixture, and then forming the mixture into uniform spheres using a catalyst spherical molding device to obtain a spherical mixture with a diameter of 2 mm;
[0126] (4) The spherical mixture in step (3) is placed at room temperature for 5 days, and then placed in an oven at a temperature of 160°C for drying for 18 hours, and then transferred to a carbonization converter for calcination. Before calcination, the air is exhausted, and then nitrogen is introduced at a flow rate of 220 mL / min. The temperature is then raised to 700°C and maintained for 2.5 hours. The speed of the carbonization converter during calcination is 5 r / min. After calcination and carbonization, it is naturally cooled to room temperature to obtain a crude catalyst product (i.e., sludge charcoal).
[0127] (5) At room temperature and sealed conditions, the crude catalyst product obtained in step (4) was immersed in a 5% mass concentration oxalic acid solution for activation treatment for 12 hours; then rinsed with ultrapure water until the eluent was neutral, placed in an oven at 110° C. for 20 hours, and cooled to obtain the catalyst YCC-M (4) of this example.
[0128] application:
[0129] The wastewater from the biochemical secondary effluent section of a coking wastewater in an industrial park was taken as the treatment object (i.e., raw water). The wastewater was light yellow, had a pungent odor, a pH of 4, a COD of 295 mg / L, a TOC of 120 mg / L, and NH4 + -N is 25 mg / L, and the mass concentration of chloride ions is 3%. The catalyst YCC-M (4) of this example is used to carry out CWPO advanced oxidation treatment on the wastewater. The reaction conditions are: temperature 30°C, pH 5, hydrogen peroxide 0.5 kg / t (30 wt.%) and reactor space velocity 1 h -1 A control experiment 4 was set up, that is, no catalyst was added in the CWPO reaction stage, and other reaction conditions were the same; at the same time, the existing commercial catalyst Fe(II)@ZSM-5 was used instead of the catalyst of this example to carry out CWPO advanced oxidation treatment, and other reaction conditions were the same. The inlet and outlet water quality analysis and testing items involved chemical oxygen demand (COD), total organic carbon (TOC), ammonia nitrogen (NH4 +-N) etc. After adding the catalyst of this example, the CWPO treatment device (which is a conventional reaction device of CWPO, the specific structure is not repeated here) is allowed to run stably for a period of time until the effluent quality is stable, and the result is recorded in Table 4.
[0130] Table 4 Wastewater treatment effects of the catalyst of Example 4, control experiment 4, and commercial catalyst Fe(II)@ZSM-5
[0131]
[0132] It can be seen from Table 4 that when treating coking wastewater of the same water quality, the effluent water quality of the catalyst YCC-M (4) of this embodiment is significantly improved, especially the COD removal rate, compared with the case where no catalyst is added or the catalyst is commercial Fe (II) @ ZSM-5. At the same time. It can also be seen from Tables 2-4 that the catalyst of the present application has a good effect on the treatment of coking wastewater of different water qualities, and is better than the commercial Fe (II) @ ZSM-5 catalyst and the control experimental group.
[0133] Comparative Example 1
[0134] This comparative example is substantially the same as Example 4, except that:
[0135] The preparation method of the catalyst of this comparative example does not carry out the step of oxalic acid activation, that is, does not carry out step (5), and the prepared catalyst is marked as catalyst YCC-0.
[0136] During the application process, the case of treating wastewater without adding a catalyst is referred to as control experiment 5 (control experiment 5 is only for the convenience of expression to distinguish it from control experiment 4, which are essentially the same experiments).
[0137] When the catalyst of this comparative example, control experiment 5 without adding a catalyst, and commercial catalyst Fe(II)@ZSM-5 were used for treatment, the treatment results are shown in Table 5.
[0138] Table 5 Wastewater treatment effects of the catalyst of comparative example 1, control experiment 5, and commercial catalyst Fe(II)@ZSM-5
[0139]
[0140] It can be seen from Table 5 that when treating coking wastewater of the same water quality, compared with the case where no catalyst is added or the catalyst is commercial Fe(II)@ZSM-5, the effluent water quality of the catalyst YCC-0 in this comparative example is higher than that of the control experimental group (only about 8% higher than the treatment effect of the control group), but significantly lower than that of the commercial Fe(II)@ZSM-5 catalyst. At the same time, it can be seen from Tables 4 and 5 that if the catalyst of the present application is not activated by oxalic acid, its effect on treating coking wastewater is greatly reduced, with a COD removal rate reduction of nearly 40%, a TOC removal rate reduction of 35%, and a NH4 + -N removal rate decreased by 50%.
[0141] Comparative Example 2
[0142] This comparative example is substantially the same as Example 4, except that:
[0143] In the preparation method of the catalyst of this comparative example, no yellow sandstone is added, and the prepared catalyst is marked as catalyst CSC-M.
[0144] During the application process, the case of treating wastewater without adding a catalyst is referred to as control experiment 6 (control experiment 6 is only for the convenience of expression to distinguish it from control experiment 4, which are essentially the same experiments).
[0145] When the catalyst of this comparative example, control experiment 6 without adding a catalyst, and the commercial catalyst Fe(II)@ZSM-5 were used for treatment, the treatment results are shown in Table 6.
[0146] Table 6 Wastewater treatment effects of the catalyst of comparative example 2, control experiment 6, and commercial catalyst Fe(II)@ZSM-5
[0147]
[0148] It can be seen from Table 6 that without adding yellow sandstone, the coking wastewater treatment effect of the catalyst in this comparative example is significantly higher than that of the control experimental group, and slightly lower than that of the commercial catalyst Fe(II)@ZSM-5. At the same time, it can be seen from Tables 4 and 6 that without adding yellow sandstone, the coking sludge carbon catalyst (that is, the catalyst of comparative example 2) prepared with coking sludge as raw material has a much lower degradation effect on coking wastewater than the yellow sandstone modified coking sludge carbon catalyst prepared in this application (that is, the catalyst of Example 4), wherein the COD removal rate is reduced by 20%, TOD is reduced by 16.6%, and NH4 + -N removal rate decreased by 50%.
[0149] The elemental composition, specific surface area and pore volume of the yellow sandstone in Example 4, the coking sludge in Example 4, the catalyst of Comparative Example 1, the catalyst of Comparative Example 1 and the catalyst of Example 4 were tested, and the results are shown in Table 7.
[0150] Table 7 Elemental composition, specific surface area and pore volume of the catalysts of yellow sandstone, coking sludge, comparative examples 1-2 and example 4
[0151]
[0152] Note: YSS is the yellow sandstone in Example 4; CSS is the coking sludge in Example 4; CSC-M is the coking sludge charcoal activated with oxalic acid in Comparative Example 2 (the catalyst of Comparative Example 2); YCC-0 is the yellow sandstone modified coking sludge charcoal without oxalic acid activation in Comparative Example 1 (the catalyst of Comparative Example 1); YCC-M(4) is the yellow sandstone modified coking sludge charcoal activated with oxalic acid in Example 4 (the catalyst of Example 4).
[0153] It can be seen from Table 7 that compared with the catalysts of Comparative Examples 1 and 2, the catalyst of Example 4 has higher specific surface area and pore volume, wherein the specific surface area of the catalyst of Example 4 is 17.8 times that of the catalyst of Comparative Example 1 which is not activated with oxalic acid, and the pore volume of the catalyst of Example 4 is 10.9 times that of the catalyst of Comparative Example 1 which is not activated with oxalic acid, indicating that oxalic acid activation can effectively increase the specific surface area and pore volume of the catalyst.
[0154] Comparative Example 3
[0155] This comparative example is substantially the same as Example 4, except that:
[0156] In the preparation method of the catalyst of this comparative example, nitric acid is used instead of oxalic acid in the impregnation activation process.
[0157] During the application process, the case of treating wastewater without adding a catalyst is referred to as control experiment 7 (control experiment 7 is only for the convenience of expression to distinguish it from control experiment 4, which are essentially the same experiments).
[0158] When the catalyst of this comparative example, control experiment 7 without adding a catalyst, and the commercial catalyst Fe(II)@ZSM-5 were used for treatment, the treatment results are shown in Table 8.
[0159] Table 8 Wastewater treatment effects of the catalyst of comparative example 3, control experiment 7, and commercial catalyst Fe(II)@ZSM-5
[0160]
[0161] It can be seen from Table 8 that the treatment effect of comparative example 3 on coking wastewater is relatively poor. This is because nitric acid is a strong acid and has a great destructive effect on the strength of sludge charcoal. After use, the sludge charcoal becomes powder.
[0162] Examples 5-16 and Comparative Examples 4-10 are substantially the same as Example 4, except that some parameters in the catalyst preparation method are designed differently, as shown in Table 9.
[0163] Table 9 Partial parameter design of Examples 4-16 and Comparative Examples 4-10
[0164]
[0165] The catalyst wastewater treatment effects of Example 4-16 and Comparative Example 4-10 are shown in Table 10.
[0166] Table 10 Catalyst wastewater treatment effects of Examples 4-16 and Comparative Examples 4-10
[0167]
[0168]
[0169] It can be seen from Table 10 that when the values of the process parameters are within the range of values corresponding to this application, the catalyst of this application has a good effect on the coking wastewater (pH is 4, COD is 295 mg / L, TOC is 120 mg / L, NH 4+ -N is 25mg / L) all have good treatment effects, among which the COD removal rate is mostly above 60%, the TOD removal rate is mostly above 50%, and the NH 4+ -N removal rates were mostly above 4%; in contrast, when both the first organic acid and the second organic acid were oxalic acid, the removal rates of COD and TOD were higher. When the values of the process parameters exceeded the value ranges corresponding to this application, in most cases, COD, TOD and NH 4+ -N removal rates decreased significantly.
[0170] In summary, the catalyst prepared by the catalyst preparation method of the present application has a good effect in treating coking wastewater, the dissolution rate of the active components of the catalyst is low, the catalyst properties are stable, and the service life is long. The use of yellow sandstone to modify the sludge and activate it with oxalic acid, etc. plays an important role in improving the catalytic activity and stability of the sludge charcoal.
[0171] In this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0172] In addition, the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" and the like mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0173] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A method for preparing a catalyst, characterized in that: include: The yellow sandstone is mixed with the sludge, and after first drying, a first organic acid is added to prepare a granular mixture; The granular mixture is allowed to stand, dried, and then calcined under an inert atmosphere to obtain a crude catalyst product; The crude catalyst product is impregnated and activated, followed by impurity removal and secondary drying to obtain the catalyst product; The sludge is iron-containing sludge; The mass ratio of the yellow sandstone to the sludge is (1:10)-(1:8); The calcination is carried out in an oxygen-free environment at a temperature of 600-800°C; The impregnation liquid for impregnation activation is a second organic acid, and the second organic acid is a medium-strong acid.
2. The preparation method according to claim 1, characterized in that: The yellow sandstone is yellow sandstone containing 3-5wt% of jarosite mineral; and / or, the yellow sandstone needs to be ground and sieved before being mixed with the sludge; And / or, the sludge is one or more of coking wastewater sludge, petrochemical wastewater sludge, and pharmaceutical wastewater sludge; and / or, the first organic acid is one or more of oxalic acid, acetic acid, and formic acid; And / or, the mass concentration of the first organic acid is 4-6%, and the added amount of the first organic acid is 0.3-0.6% of the total mass of the yellow sandstone and the sludge after the first drying.
3. The preparation method according to claim 2, characterized in that: The coking wastewater sludge is sludge with a moisture content of 75-80% discharged from the reclaimed water treatment link in the coking wastewater treatment plant.
4. The preparation method according to claim 1, characterized in that: The first drying includes natural air drying and / or oven drying; And / or, the standing temperature is room temperature, the standing time is 3-5 days, the drying temperature is 150-170° C., and the drying time is 12-24 hours.
5. The preparation method according to claim 4, characterized in that: The natural air drying time is 5-7 days; And / or, the oven drying temperature is 105-120° C., and the oven drying time is 24-36 hours.
6. The preparation method according to claim 1, characterized in that: The calcination time is 2-3h; And / or, the roasting is carried out in a carbonizing converter, and the rotation speed of the carbonizing converter during the roasting process is 3-8 r / min; And / or, the flow rate of the inert atmosphere during the calcination process is 200-300 mL / min.
7. The preparation method according to claim 1, characterized in that: The second organic acid is one or more of oxalic acid, acetic acid, and formic acid; And / or, the impregnation activation is carried out under sealed conditions, the temperature of the impregnation activation is room temperature, and the time of the impregnation activation is 10-15 hours.
8. The preparation method according to claim 1, characterized in that: The impurity removal method is to use ultrapure water to rinse until the eluent is neutral; And / or, the drying temperature of the second drying is 105-120° C., and the drying time of the second drying is 24-36 hours.
9. A catalyst, characterized in that The method is prepared according to any one of claims 1 to 8.
10. Use of the catalyst as claimed in claim 9 in water treatment.
Citation Information
Patent Citations
Municipal wastewater purification treatment method
CN103755108A
Preparation method of sludge char catalyst as well as catalyst and application
CN106311202A
Industrial wastewater treatment process of zero-valent iron internal electrolysis coupled internal circulating fluidized bed Fenton
CN109455796A
Technology for treating fracturing flow-back fluid of oil and gas field through multi-metal catalytic oxidation
CN110550814A
Ship exhaust gas purification apparatus and method
CN114096744A