A positive electrode material precursor and its preparation method and application

By using fluorine-doped nickel-ferromanganese-aluminum hydroxide core and nickel-cobalt-aluminum hydroxide shell in the positive electrode material of lithium-ion battery, the existing technology is solved by combining the rare earth oxide functional coating. The problem of insufficient rate and cycle performance of the cathode material significantly improves the electrochemical performance and stability of the material.

CN116239162BActive Publication Date: 2024-11-22SVOLT ENERGY TECH (WUXI) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310338631.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-11-22
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

The current lithium-ion battery positive electrode materials have insufficient rate performance in fast charging systems, and the circulation performance and high temperature stability need to be improved.

Method used

Using fluorine and nitrogen-doped nickel iron-manganese aluminum hydroxide as the core, and the outer shell is fluorine and nitrogen-doped nickel cobalt aluminum hydroxide. The precursor of the double-layer structure positive electrode material is prepared by co-precipitation method and set on the surface of the material. Rare earth oxide functional coating.

Benefits of technology

It improves the circulation and rate performance of the material, enhances structural stability and electrochemical properties, inhibits acidic HF erosion and interface instability, and shows good cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116239162B_ABST
    Figure CN116239162B_ABST
Patent Text Reader

Abstract

The present invention discloses a positive electrode material precursor and a preparation method and application thereof. The positive electrode material precursor comprises a core and a shell coated on the surface of the core, wherein the core is nickel-iron-manganese-aluminum hydroxide doped with fluorine and nitrogen, and the shell is nickel-cobalt-aluminum hydroxide doped with fluorine and nitrogen. In the positive electrode material precursor of the present invention, the shell contains cobalt element, which can stabilize the layered structure of the material and improve the cycle and rate performance of the material, and the aluminum element can improve the safety performance and structural stability of the material. Further addition of fluorine and nitrogen to the inner core and the outer core is conducive to the refinement of the primary particles, making the material more compact, further enhancing the structural stability, and improving the electrochemical performance of the material. The positive electrode material precursor is used to prepare the positive electrode active material and a rare earth oxide functional coating is provided on its surface, so that the battery has excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials and relates to a positive electrode material precursor and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have been widely used in mobile phones, laptops and electric vehicles due to their good cycle stability, environmental protection and high energy density. With the deepening of application, people have put forward higher requirements for the cycle performance and rate performance of lithium-ion batteries, and researchers have devoted themselves to a lot of discussion and research on this.

[0003] CN103117387A discloses a method for preparing lithium nickel manganese aluminum oxide, a positive electrode material for lithium ion batteries. The method comprises the following steps: using a spherical nickel manganese aluminum composite oxide or carbonate prepared by a coprecipitation method as a raw material, subjecting the nickel manganese composite hydroxide or carbonate to oxidation and calcination treatment to obtain a high-valent spherical nickel manganese oxide uniform solid solution in advance, uniformly mixing the pre-oxidized high-valent nickel manganese oxide with a lithium salt, calcining at high temperature in an oxygen atmosphere, and cooling and crushing to obtain a spherical lithium nickel manganese aluminum oxide positive electrode material. The prepared spherical lithium nickel manganese aluminum oxide positive electrode material has uniform particle distribution, large discharge specific capacity, good cycle performance, simple preparation process, and low cost.

[0004] CN105322151A discloses a method for preparing a modified lithium-ion battery positive electrode material, lithium nickel manganese oxide, which is prepared by mixing manganese salt and nickel salt materials through a sol-gel method to prepare a nickel manganese precursor, and the nickel manganese precursor is mixed with a lithium salt using a three-dimensional oblique mixer, and then pre-sintered and high-temperature sintered, and then doped with F- or F- and metal cations, and then metal oxides are added for wet coating, and finally low-temperature sintering, airflow crushing and classification are performed to obtain a finished product of lithium nickel manganese oxide. This method improves the cycle performance and high-temperature stability of lithium nickel manganese oxide by ion doping modification technology, and improves the high-voltage cycle performance and high-temperature stability of lithium nickel manganese oxide by wet coating technology. However, this material is not suitable for fast charging systems, and the rate performance needs to be improved.

[0005] Therefore, it is necessary to provide a high-performance cathode material that has both excellent rate performance and good rate performance. Summary of the invention

[0006] In view of the above problems existing in the prior art, the object of the present invention is to provide a positive electrode material precursor and a preparation method and application thereof.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a positive electrode material precursor, comprising a core and a shell coated on the surface of the core, wherein the core is nickel-iron-manganese-aluminum hydroxide doped with fluorine and nitrogen, and the shell is nickel-cobalt-aluminum hydroxide doped with fluorine and nitrogen.

[0009] The cathode material precursor of the present invention has fluorine and nitrogen doped nickel iron manganese aluminum hydroxide as the core, the surface of the core is coated with fluorine and nitrogen doped nickel cobalt aluminum hydroxide, the shell contains cobalt element, which can stabilize the layered structure of the material, improve the material's cycle and rate performance, and the aluminum element in the core and shell can improve the material's safety performance and structural stability. Further fluorine and nitrogen are added to the core and outer core, which is conducive to the refinement of primary particles, making the material more dense, further enhancing the structural stability, and improving the electrochemical performance of the material.

[0010] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0011] Preferably, the chemical formula of the core is Ni x1 Fe y1 Mn z1 Al h1 (OH) 2-a1-b1 F a1 N b1 , 0.1≤x1≤0.9, 0.05≤y1≤0.3, 0.05≤z1≤0.3, 0.05≤h1≤0.3, x1+y1+z1+h1=1, 0.01≤a1≤0.2, 0.01≤b1≤0.2. Exemplarily, x1 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, y1 can be, for example, 0.05, 0.07, 0.1, 0.15, 0.2, 0.25 or 0.3, z1 can be, for example, 0.05, 0.07, 0.1, 0.15, 0.2, 0.25 or 0.3, h1 can be, for example, 0.05, 0.07, 0.1, For example, a1 can be 0.01, 0.02, 0.05, 0.07, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.2, and b1 can be 0.01, 0.02, 0.03, 0.05, 0.06, 0.07, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.2, etc.

[0012] Preferably, the chemical formula of the shell is Ni x3 Co y3 Al z3 (OH)2-a2-b2 F a2 N b2 , 0.1≤x3≤0.8, 0.1≤y3≤0.8, 0.1≤z3≤0.8, x3+y3+z3=1, 0.01≤a2≤0.2, 0.01≤b2≤0.2. Exemplarily, x3 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8, y3 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8, a2 can be, for example, 0.01, 0.03, 0.05, 0.07, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.2, and b2 can be, for example, 0.01, 0.03, 0.05, 0.07, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.2, etc.

[0013] Preferably, the particle size D50 of the inner core is 3 μm to 6 μm, for example, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm or 6 μm.

[0014] Preferably, the particle size D50 of the positive electrode material precursor is 10 μm to 15 μm, for example, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm or 15 μm.

[0015] In a second aspect, the present invention provides a method for preparing a positive electrode material precursor as described in the first aspect, the method comprising the following steps:

[0016] (a) Solution preparation:

[0017] A mixed metal salt solution A is prepared by using nickel salt, iron salt, manganese salt and aluminum salt;

[0018] A mixed metal salt solution B is prepared by using nickel salt, cobalt salt and aluminum salt;

[0019] preparing a precipitant solution, a complexing agent solution, a fluorine source solution and a nitrogen source solution;

[0020] (b) Coprecipitation reaction:

[0021] A mixed metal salt solution A, a precipitant solution, a complexing agent solution, a fluorine source solution and a nitrogen source solution are introduced into a reaction container containing a base liquid to carry out a first coprecipitation reaction. After obtaining an inner core of a preset particle size, the mixed metal salt solution A is replaced with a mixed metal salt solution B, and a second coprecipitation reaction is continued to obtain the positive electrode material precursor.

[0022] In the method of the present invention, the preparation order of the solutions in step (a) is not limited, that is, the preparation order of the mixed metal salt solution A, the mixed metal salt solution B, the precipitant solution, the complexing agent solution, the fluorine source solution and the nitrogen source solution is not limited, and they can be prepared simultaneously or separately, and when they are prepared separately, the preparation of each solution is not prioritized.

[0023] The method of the invention can uniformly dope fluorine and nitrogen elements in the inner core and the outer shell, the doping uniformity is good, and the doping amount is controllable.

[0024] As a preferred technical solution of the method of the present invention, the concentration of the mixed metal salt solution A in step (a) is 0.5 mol / L to 3 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L.

[0025] Preferably, the concentration of the mixed metal salt solution B in step (a) is 0.7 mol / L to 4.0 mol / L, for example, 0.7 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L.

[0026] Preferably, the fluorine source in the fluorine source solution in step (a) comprises at least one of sodium fluoride, potassium fluoride and magnesium fluoride;

[0027] Preferably, the nitrogen source in the nitrogen source solution in step (a) comprises at least one of sodium nitride, potassium nitride and magnesium nitride.

[0028] As a preferred technical solution of the method of the present invention, the pH value of the base solution in step (b) is 11.8-12.2, for example, 11.8, 11.9, 12.0, 12.1 or 12.2.

[0029] Preferably, the base solution in step (b) comprises a precipitant and a complexing agent.

[0030] Preferably, the ammonia concentration in the base solution in step (b) is 3 g / L to 5 g / L, for example, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or 5 g / L.

[0031] Preferably, during the entire reaction process of step (b), the reaction temperature is in the range of 50°C to 70°C (for example), the pH value of the reaction system is in the range of 11 to 13, and the reaction is accompanied by stirring, and the stirring speed is preferably in the range of 200rpm to 800rpm.

[0032] In the present invention, the entire reaction process of step (b) includes both the first coprecipitation reaction and the second coprecipitation reaction. The settings of the parameters in the first coprecipitation reaction and the second coprecipitation reaction can be the same or different. For example, the reaction temperature, pH value, stirring speed, concentration of the precipitant, concentration of the complexing agent, concentration of fluoride ions and concentration of nitrogen ions can be completely consistent, or at least one of the above items can be different. That is, the selection of the parameters in the first coprecipitation reaction and the second coprecipitation reaction is independent of each other.

[0033] Illustratively, the reaction temperature may be, for example, 50°C, 55°C, 60°C, 65°C or 70°C, etc.; the pH value may be, for example, 11, 11.5, 12 or 13, etc.; the stirring speed may be, for example, 200rpm, 300rpm, 400rpm, 500rpm, 600rpm, 700rpm or 800rpm, etc.

[0034] Preferably, during the entire reaction process of step (b), the concentration of the precipitant in the reaction system is 2.0 mol / L to 10.0 mol / L, such as 2.0 mol / L, 3.0 mol / L, 4.0 mol / L, 5.0 mol / L, 6.0 mol / L, 7.0 mol / L, 8.0 mol / L, 9.0 mol / L or 10.0 mol / L, etc.; the concentration of the complexing agent is 4.0 mol / L to 15.0 mol / L, such as 4.0 mol / L, 5.0 mol / L, 6.0 mol / L, 8.0 mol / L, 10.0 mol / L, 11.0 mol / L, 13.0 mol / L or 15.0 mol / L, etc.

[0035] The present invention does not limit the types of the precipitant and the complexing agent. For example, the precipitant may be sodium hydroxide, and the complexing agent may be aqueous ammonia.

[0036] Preferably, during the entire reaction process of step (b), the concentration of fluoride ions in the reaction system is in the range of 0.5 mmol / L to 2.0 mmol / L, and the concentration of nitrogen ions is in the range of 0.5 mmol / L to 2.0 mmol / L. For example, the concentration of fluoride ions may be, for example, 0.5 mmol / L, 1 mmol / L, 1.5 mmol / L or 2.0 mmol / L, and the concentration of nitrogen ions may be, for example, 0.5 mmol / L, 1 mmol / L, 1.5 mmol / L or 2.0 mmol / L, and the like.

[0037] Preferably, in step (b), the flow rate of the mixed metal salt solution B is greater than the flow rate of the mixed metal salt solution A.

[0038] Preferably, the flow rate difference between the inlet flow rate of the mixed metal salt solution B and the inlet flow rate of the mixed metal salt solution A is 50L / h to 300L / h, for example, 50L / h, 60L / h, 70L / h, 80L / h, 90L / h, 100L / h, 110L / h, 120L / h, 130L / h, 150L / h, 170L / h, 180L / h, 200L / h, 220L / h, 240L / h, 260L / h, 280L / h or 300L / h, etc.

[0039] Preferably, the flow rate of the mixed metal salt solution A is 60L / h to 300L / h, for example, 60L / h, 70L / h, 80L / h, 100L / h, 115L / h, 130L / h, 150L / h, 160L / h, 180L / h, 200L / h, 230L / h, 260L / h, 280L / h or 300L / h, etc.

[0040] Preferably, the flow rate of the mixed metal salt solution B is 200L / h to 600L / h, for example, 200L / h, 220L / h, 240L / h, 260L / h, 280L / h, 300L / h, 350L / h, 400L / h, 450L / h, 500L / h, 550L / h or 600L / h, etc.

[0041] Preferably, the method further comprises the step of introducing a protective gas into the reaction container, and the oxygen concentration in the reaction container is 0% to 8%, such as 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8%, etc. By introducing the protective gas, oxidation can be prevented, which is beneficial to improving the performance of the positive electrode material.

[0042] Preferably, the flow rate of the protective gas is 10L / min to 500L / min, for example, 10L / min, 20L / min, 40L / min, 60L / min, 80L / min, 100L / min, 125L / min, 150L / min, 170L / min, 200L / min, 220L / min, 240L / min, 260L / min, 280L / min, 300L / min, 350L / min, 400L / min, 450L / min or 500L / min, etc.

[0043] In a third aspect, the present invention provides a positive electrode active material, which is prepared using the positive electrode material precursor described in the first aspect, and the positive electrode active material includes nickel-iron-manganese-aluminum oxide and nickel-cobalt-aluminum oxide arranged in the nickel-iron-manganese-aluminum oxide, the nickel-iron-manganese-aluminum oxide is doped with fluorine and nitrogen, and the nickel-cobalt-aluminum oxide is doped with fluorine and nitrogen.

[0044] Preferably, the outer surface of the nickel-cobalt-aluminum oxide is provided with a rare earth oxide functional coating.

[0045] Preferably, the rare earth oxide includes at least one of Gd2O3, Y2O3 and Sc2O3.

[0046] In the positive electrode active material of the present invention, the rare earth oxide functional coating acts as a passivation film, which can block the direct contact between the electrode and the electrolyte, prevent acidic HF from corroding the positive electrode material, and further inhibit the dissolution of active transition metal ions and the oxidative decomposition of the electrolyte; at the same time, the rare earth oxide functional coating acts as an electron reservoir, which can enhance the electron and ion transmission capacity of the material, improve the rate performance, and at the same time, it can also be unstable Ni 4+ Charge compensation is performed to prevent it from plundering electrons from lattice oxygen, thereby inhibiting the loss of interface lattice oxygen and the occurrence of harmful interface phase transitions, showing good cycle stability.

[0047] In a fourth aspect, the present invention provides a method for preparing a positive electrode active material as described in the third aspect, the method comprising the following steps: mixing a positive electrode material precursor and a lithium source, and performing a first heat treatment to obtain a positive electrode active material.

[0048] The present invention does not specifically limit the type of lithium source, including but not limited to lithium hydroxide or lithium carbonate.

[0049] Preferably, the temperature of the first heat treatment is 600°C to 900°C, for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or 900°C.

[0050] Preferably, the first heat treatment time is 6 h to 20 h, for example, 6 h, 8 h, 10 h, 12 h, 13 h, 15 h, 18 h or 20 h.

[0051] Preferably, the first heat treatment is performed in an oxygen atmosphere.

[0052] Preferably, during the first heat treatment, the gas flow rate of the oxygen atmosphere is 0.2 m 3 / h~2.0m 3 / h, for example 0.2m 3 / h、0.5m 3 / h、0.8m 3 / h、1.0m 3 / h、1.3m 3 / h、1.6m 3 / h、1.8m 3 / h or 2.0m 3 / h, etc.

[0053] Preferably, the first heat treatment is performed by microwave heating.

[0054] As a preferred technical solution of the method of the present invention, the method also includes the step of coating the positive electrode active material, specifically including: mixing the positive electrode material and the rare earth oxide, and then performing a second heat treatment to obtain the positive electrode material with a coating layer.

[0055] Preferably, the molar ratio of the rare earth oxide to the positive electrode active material is (0.01-0.1):1, for example, 0.01:1, 0.02:1, 0.03:1, 0.05:1, 0.07:1, 0.08:1 or 0.1:1, etc.

[0056] Preferably, the temperature of the second heat treatment is 600°C to 900°C, for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or 900°C.

[0057] Preferably, the second heat treatment time is 5 h to 20 h, for example, 5 h, 6 h, 8 h, 10 h, 12 h, 14 h, 15 h, 17 h, 18 h or 20 h.

[0058] Preferably, the second heat treatment is performed in an oxygen atmosphere.

[0059] Preferably, in the second heat treatment, the gas flow rate of the oxygen atmosphere is 0.1 m 3 / h~2.0m 3 / h, for example 0.2m 3 / h、0.5m 3 / h、0.8m 3 / h、1.0m 3 / h、1.3m 3 / h、1.6m 3 / h、1.8m 3 / h or 2.0m 3 / h, etc.

[0060] As a preferred technical solution of the method of the present invention, the positive electrode material is preliminarily washed before being mixed with the rare earth oxide.

[0061] Preferably, the detergent used in the washing treatment is deionized water.

[0062] Preferably, during the washing process, the mass ratio of deionized water to the positive electrode material is (1-2):1, such as 1:1, 1.2:1, 1.4:1, 1.5:1, 1.7:1 or 2:1, etc. The washing time is 5 min to 30 min, such as 5 min, 8 min, 10 min, 12 min, 15 min, 18 min, 20 min, 25 min or 30 min, etc.

[0063] Preferably, the washing process is followed by a drying process.

[0064] Preferably, the drying treatment is: drying in a rotary vacuum drying furnace, the rotation speed of the rotary vacuum drying furnace is 60r / min to 200r / min, for example, 60r / min, 80r / min, 100r / min, 120r / min, 140r / min, 160r / min, 180r / min or 200r / min, etc.

[0065] In a third aspect, the present invention provides a lithium ion battery, wherein the positive electrode of the lithium ion battery comprises the positive electrode active material described in the third aspect.

[0066] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0067] Compared with the prior art, the present invention has the following beneficial effects:

[0068] (1) The cathode material precursor of the present invention has a fluorine and nitrogen doped nickel iron manganese aluminum hydroxide as the core, the surface of the core is coated with fluorine and nitrogen doped nickel cobalt aluminum hydroxide, and the shell contains cobalt elements, which can stabilize the layered structure of the material and improve the material's cycle and rate performance. The aluminum elements in the core and shell can improve the material's safety performance and structural stability. Further fluorine and nitrogen in the core and outer core are conducive to the refinement of primary particles, making the material more dense, further enhancing the structural stability, and improving the electrochemical performance of the material.

[0069] (2) The positive electrode material precursor of the present invention is used to prepare a positive electrode active material and a rare earth oxide functional coating is provided on the surface of the positive electrode active material. The rare earth oxide functional coating acts as a passivation film, which can block the direct contact between the electrode and the electrolyte, prevent acidic HF from corroding the positive electrode material, and further inhibit the dissolution of active transition metal ions and the oxidative decomposition of the electrolyte; at the same time, the rare earth oxide functional coating acts as an electron reservoir, which can enhance the electron and ion transmission capacity of the material, improve the rate performance, and can also 4+Charge compensation is performed to prevent it from plundering electrons from lattice oxygen, thereby inhibiting the loss of interface lattice oxygen and the occurrence of harmful interface phase transitions, showing good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 This is a schematic diagram of the structure of the positive electrode active material of Application Example 1 of the present invention. Figure 1 . DETAILED DESCRIPTION

[0071] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0072] Example 1

[0073] This embodiment provides a double-layer structured cathode material precursor, the preparation method of which includes the following steps:

[0074] (a) Solution preparation:

[0075] Nickel sulfate, iron sulfate, manganese sulfate and aluminum sulfate were prepared into a mixed metal salt solution A with deionized water in a molar ratio of 8:1:0.5:0.5, and the total metal ion concentration was 2 mol / L.

[0076] Nickel sulfate, cobalt sulfate, aluminum sulfate and deionized water were prepared into metal salt solution B in a molar ratio of 8:1:1, and the total concentration of metal ions was 1 mol / L.

[0077] Prepare 11 mol / L sodium hydroxide solution, 11 mol / L ammonia water, 1.5 mmol / L sodium fluoride solution and 1.5 mmol / L sodium nitride solution.

[0078] (b) Preparation of reaction kettle bottom liquid:

[0079] Add deionized water to the reactor to 1 / 2 of its volume, stir at 260 rpm, control the temperature at 60°C, add the above-mentioned sodium hydroxide solution and ammonia water, adjust the pH value to 11.9, and the ammonia concentration to 4 g / L to prepare the reactor bottom liquid, and introduce nitrogen into the reactor.

[0080] (c) First coprecipitation complex reaction:

[0081] The mixed metal salt solution A, sodium fluoride solution, sodium nitride solution, sodium hydroxide solution and ammonia water are continuously added to the stirred reactor through their respective liquid inlet pipes, the temperature of the reaction system is controlled to be 60±0.3°C, the pH value is 12.1, the ammonia concentration is 4g / L, the gas flow rate of the nitrogen atmosphere is 30L / min, the reaction time is 16h, and when the reaction reaches the desired particle size (the particle size D50 of the inner core is 4μm), the mixed metal salt solution A is stopped from being pumped in;

[0082] The reaction was accompanied by stirring at a speed of 300 rpm, and the flow rate of the mixed metal salt solution A was 100 L / h; the concentration of sodium hydroxide in the reaction system was 5 mol / L, the concentration of NH3 was 10 mol / L, the concentration of fluoride ions was 1 mmol / L, and the concentration of nitrogen ions was 1 mmol / L.

[0083] (d) Second coprecipitation complex reaction:

[0084] Continue to add sodium fluoride solution, sodium nitride solution, sodium hydroxide solution and ammonia water to the stirred reactor through their respective liquid inlet pipes, stop pumping solution A, and pump in mixed metal salt solution B; control the temperature of the reaction system to 60±0.3°C, pH value to 12.5, ammonia concentration to 8g / L, and nitrogen atmosphere gas flow rate to 100L / min. When the reaction reaches the desired particle size (the particle size D50 of the double-layer structure cathode material precursor is 10μm), filter the obtained precursor slurry, wash the solid product, place it in a vacuum drying oven at 120°C and dry it for 10h, sieve it with a 400-mesh screen, remove iron, and obtain a double-layer structure cathode material precursor;

[0085] The reaction was accompanied by stirring at a speed of 400 rpm, and the flow rate of the mixed metal salt solution B was 200 L / h; the concentration of sodium hydroxide in the reaction system was 5 mol / L, the concentration of NH3 was 10 mol / L, the concentration of fluoride ions was 1 mmol / L, and the concentration of nitrogen ions was 0.5 mmol / L.

[0086] The double-layer positive electrode material precursor prepared in this embodiment includes a core and a shell coated on the surface of the core. The chemical formula of the core is Ni 0.8 Fe 0.1 Mn 0.05 Al 0.05 (OH) 1.6 F 0.2 N 0.2 , the chemical formula of the shell is Ni 0.8 Co 0.1 Al 0.1 (OH) 1.6 F 0.2 N 0.2 .

[0087] Example 2

[0088] This embodiment provides a double-layer structured cathode material precursor, the preparation method of which includes the following steps:

[0089] (a) Solution preparation:

[0090] Nickel sulfate, iron sulfate, manganese sulfate and aluminum sulfate were prepared into a mixed metal salt solution A with deionized water in a molar ratio of 7.5:1:0.5:1, and the total concentration of metal ions was 1 mol / L.

[0091] Nickel sulfate, cobalt sulfate, aluminum sulfate and deionized water were prepared into metal salt solution B in a molar ratio of 8:1:1, and the total concentration of metal ions was 2 mol / L.

[0092] Prepare 10 mol / L sodium hydroxide solution, 8 mol / L ammonia water, 1.0 mmol / L sodium fluoride solution and 1.0 mmol / L sodium nitride solution.

[0093] (b) Preparation of reaction kettle bottom liquid:

[0094] Add deionized water to the reactor to 1 / 2 of its volume, stir at 500 rpm, control the temperature at 70°C, add the above-mentioned sodium hydroxide solution and ammonia water, adjust the pH value to 12.5, and the ammonia concentration to 10 g / L to prepare the reactor bottom liquid, and introduce nitrogen into the reactor.

[0095] (c) First coprecipitation complex reaction:

[0096] The mixed metal salt solution A, sodium fluoride solution, sodium nitride solution, sodium hydroxide solution and ammonia water are continuously added to the stirred reactor through their respective liquid inlet pipes, and the temperature of the reaction system is controlled to be 65±0.3°C, the pH value is 12.5, the ammonia concentration is 10g / L, and the gas flow rate of the nitrogen atmosphere is 50L / min. When the reaction reaches the desired particle size (the particle size D50 of the inner core is 5μm), the mixed metal salt solution A is stopped from being pumped in;

[0097] The reaction was accompanied by stirring at a speed of 400 rpm, and the flow rate of the mixed metal salt solution A was 200 L / h; the concentration of NH3 in the reaction system was 10 mol / L, the concentration of fluoride ions was 2 mmol / L, and the concentration of nitrogen ions was 0.5 mmol / L.

[0098] (d) Second coprecipitation complex reaction:

[0099] Continue to add sodium fluoride solution, sodium nitride solution, sodium hydroxide solution and ammonia water to the stirred reactor through their respective liquid inlet pipes, stop pumping solution A, and pump in mixed metal salt solution B; control the temperature of the reaction system to 65±0.3°C, pH value to 12.5, ammonia concentration to 10g / L, and nitrogen atmosphere gas flow rate to 200L / min. When the reaction reaches the desired particle size (the particle size D50 of the double-layer structure cathode material precursor is 15μm), filter the obtained precursor slurry, wash the solid product, place it in a vacuum drying oven at 100°C and dry it for 8h, sieve it with a 400-mesh screen, remove iron, and obtain a double-layer structure cathode material precursor;

[0100] The reaction was accompanied by stirring at a speed of 300 rpm, and the flow rate of the mixed metal salt solution B was 300 L / h; the concentration of NH3 in the reaction system was 10 mol / L, the concentration of fluoride ions was 0.5 mmol / L, and the concentration of nitrogen ions was 0.5 mmol / L.

[0101] The double-layer positive electrode material precursor prepared in this embodiment includes a core and a shell coated on the surface of the core. The chemical formula of the core is Ni 0.75 Fe 0.1 Mn 0.05 Al 0.1 (OH) 1.85 F 0.05 N 0.1 ; The chemical formula of the shell is Ni 0.8 Co 0.1 Al 0.1 (OH) 1.7 F 0.1 N 0.2 .

[0102] Example 3

[0103] This embodiment provides a double-layer structured cathode material precursor, the preparation method of which includes the following steps:

[0104] (a) Solution preparation:

[0105] Nickel sulfate, iron sulfate, manganese sulfate and aluminum sulfate were prepared into a mixed metal salt solution A with a molar ratio of 8.5:0.5:0.5:0.5 and deionized water, and the total metal ion concentration was 2.5 mol / L.

[0106] Nickel sulfate, cobalt sulfate, aluminum sulfate and deionized water were prepared into metal salt solution B in a molar ratio of 7:2:1, and the total metal ion concentration was 3 mol / L.

[0107] Prepare 15 mol / L sodium hydroxide solution, 12 mol / L ammonia water, 2.0 mmol / L sodium fluoride solution and 1.0 mmol / L sodium nitride solution.

[0108] (b) Preparation of reaction kettle bottom liquid:

[0109] Add deionized water to the reactor to 1 / 2 of its volume, stir at 650 rpm, control the temperature at 55°C, add the above-mentioned sodium hydroxide solution and ammonia water, adjust the pH value to 11.5, and the ammonia concentration to 12 g / L to prepare the reactor bottom liquid, and introduce nitrogen into the reactor.

[0110] (c) First coprecipitation complex reaction:

[0111] The mixed metal salt solution A, sodium fluoride solution, sodium nitride solution, sodium hydroxide solution and ammonia water are continuously added into the stirred reactor through their respective liquid inlet pipes, and the temperature of the reaction system is controlled to be 55±0.3°C, the pH value is 11.5, the ammonia concentration is 12g / L, and the gas flow rate of the nitrogen atmosphere is 200L / min. When the reaction reaches the desired particle size (the particle size D50 of the inner core is 5.5μm), the mixed metal salt solution A is stopped from being pumped in;

[0112] The reaction was accompanied by stirring at a speed of 700 rpm, and the flow rate of the mixed metal salt solution A was 260 L / h; the concentration of NH3 in the reaction system was 12 mol / L, the concentration of fluoride ions was 1.3 mmol / L, and the concentration of nitrogen ions was 0.8 mmol / L.

[0113] (d) Second coprecipitation complex reaction:

[0114] Continue to add sodium fluoride solution, sodium nitride solution, sodium hydroxide solution and ammonia water into the stirred reactor through their respective liquid inlet pipes, stop pumping solution A, and pump in mixed metal salt solution B; control the temperature of the reaction system to 55±0.3°C, pH value to 12.0, ammonia concentration to 10g / L, and nitrogen atmosphere gas flow rate to 150L / min. When the reaction reaches the desired particle size (the particle size D50 of the double-layer structure cathode material precursor is 12μm), filter the obtained precursor slurry, wash the solid product, place it in a vacuum drying oven at 80°C and dry it for 12h, sieve it with a 400-mesh screen, remove iron, and obtain a double-layer structure cathode material precursor;

[0115] The reaction was accompanied by stirring at a speed of 500 rpm, and the flow rate of the mixed metal salt solution B was 400 L / h; the concentration of NH3 in the reaction system was 10 mol / L, the concentration of fluoride ions was 0.5 mmol / L, and the concentration of nitrogen ions was 1.0 mmol / L.

[0116] The double-layer positive electrode material precursor prepared in this embodiment includes a core and a shell coated on the surface of the core. The chemical formula of the core is Ni 0.85 Fe 0.05 Mn 0.05 Al 0.05 (OH) 1.65 F 0.15 N 0.2 , the chemical formula of the shell is Ni 0.7 Co 0.2 Al 0.1 (OH) 1.8 F 0.05 N 0.15 .

[0117] Example 4

[0118] The difference from Example 1 is that the fluoride ion concentration in the reaction system during the coprecipitation reaction in step (c) is changed to 0.3 mmol / L. In the double-layer positive electrode material precursor prepared in this example, the molar ratio of the doping amount of fluorine element in the core to the total metal ions is 0.1:1.

[0119] Example 5

[0120] The difference from Example 1 is that the fluorine ion concentration in the reaction system during the coprecipitation reaction in step (c) is changed to 2.3 mmol / L. In the double-layer positive electrode material precursor prepared in this example, the doping amount of the fluorine element in the core is 0.25:1 in molar ratio to the total metal ions.

[0121] Example 6

[0122] The difference from Example 1 is that the fluorine ion concentration in the reaction system during the coprecipitation reaction in step (d) is changed to 0.3 mmol / L. In the double-layer positive electrode material precursor prepared in this example, the doping amount of the fluorine element in the outer core is 0.1:1 in molar ratio with respect to the total metal ions.

[0123] Example 7

[0124] The difference from Example 1 is that the fluoride ion concentration in the reaction system during the coprecipitation reaction in step (d) is changed to 2.3 mmol / L. In the double-layer positive electrode material precursor prepared in this example, the molar ratio of the doping amount of fluorine element in the outer core to the total metal ions is 0.25:1.

[0125] Example 8

[0126] The difference from Example 1 is that in step (c), the flow rate of the mixed metal salt solution A is 300 L / h.

[0127] Example 9

[0128] The difference from Example 1 is that in step (c), the flow rate of the mixed metal salt solution A is 60 L / h; in step (d), the flow rate of the mixed metal salt solution B is 400 L / h.

[0129] Comparative Example 1

[0130] The difference from Example 1 is that step (d) is performed first and then step (c), that is, compared with Example 1, in the obtained double-layer structured positive electrode material precursor, the compositions of the core and the shell are interchanged.

[0131] Comparative Example 2

[0132] The difference from Example 1 is that in step (c), no sodium fluoride solution and sodium nitride solution are added.

[0133] Comparative Example 3

[0134] The difference from Example 1 is that in step (d), no sodium fluoride solution and sodium nitride solution are added.

[0135] Application Example 1

[0136] This application example provides a positive electrode active material, which is prepared using the double-layer positive electrode material precursor of Example 1, and specifically includes the following steps:

[0137] (d) lithium hydroxide and a double-layer structure cathode material precursor are added to a high-speed mixer at a molar ratio of 1.1:1 and mixed evenly to obtain a mixed powder, and the mixed powder is subjected to a first heat treatment in an oxygen atmosphere with a flow rate of 1.5 m / s. 3 / h, the heat treatment temperature is 750℃, the time is 10h, and the positive electrode active material is obtained after sintering is completed and cooled.

[0138] (e) The active material in step (d) is crushed and sieved to obtain a dry powder, which is evenly mixed with Gd2O3, and subjected to a second heat treatment in an oxygen atmosphere to obtain a positive electrode substrate coated with a rare earth oxide functional coating. The molar ratio of Gd2O3 to the positive electrode material is 0.01:1, the heat treatment temperature is 600°C, the time is 8 hours, and the flow rate of the oxygen atmosphere is 1m 3 / h.

[0139] (f) The composite positive electrode material coated in step (e) is sieved through a sieve having a mesh size of 300 to obtain a final positive electrode active material.

[0140] The structural diagram of the positive electrode active material of this application example is shown in Figure 1The positive electrode active material includes an inner layer material 1, an outer layer surface 2 coated on the surface of the inner layer material 1, and a rare earth oxide functional coating 3 coated on the surface of the outer layer material 2. The chemical formula of the inner layer material 1 is LiNi 0.8 Fe 0.1 Mn 0.05 Al 0.05 O 1.6 F 0.2 N 0.2 , the chemical formula of the outer layer material 2 is LiNi 0.8 Co 0.1 Al 0.1 O 1.6 F 0.2 N 0.2 , the chemical formula of the rare earth oxide functional coating 3 is Gd2O3.

[0141] Application Example 2

[0142] This application example provides a positive electrode active material, which is prepared using the double-layer positive electrode material precursor of Example 1, and specifically includes the following steps:

[0143] (d) lithium hydroxide and a double-layer positive electrode material precursor are added to a high-speed mixer at a molar ratio of 1.05:1 and mixed evenly to obtain a mixed powder, and the mixed powder is subjected to a first heat treatment in an oxygen atmosphere with a flow rate of 0.5 m / s. 3 / h, the heat treatment temperature is 800℃, the time is 8h, and the positive electrode active material is obtained after sintering is completed and cooled.

[0144] (e) The active material in step (d) is crushed and sieved to obtain a dry powder, which is evenly mixed with Gd2O3, and subjected to a second heat treatment in an oxygen atmosphere to obtain a positive electrode substrate coated with a rare earth oxide functional coating. The molar ratio of Gd2O3 to the positive electrode material is 0.05:1, the heat treatment temperature is 750°C, the time is 6 hours, and the flow rate of the oxygen atmosphere is 1.5 m 3 / h.

[0145] (f) The composite positive electrode material coated in step (e) is sieved through a sieve having a mesh size of 300 to obtain a final positive electrode active material.

[0146] Application Example 3

[0147] This application example provides a positive electrode active material, which is prepared using the double-layer positive electrode material precursor of Example 1, and specifically includes the following steps:

[0148] (d) lithium hydroxide and a double-layer structure cathode material precursor were added to a high-speed mixer at a molar ratio of 1.03:1 and mixed thoroughly to obtain a mixed powder. The mixed powder was subjected to a first heat treatment in an oxygen atmosphere with a flow rate of 1.5 m / s. 3 / h, the heat treatment temperature is 600℃, the time is 18h, and the positive electrode active material is obtained after sintering is completed and cooled.

[0149] (e) The active material in step (d) is crushed and sieved to obtain a dry powder, which is evenly mixed with Y2O3, and subjected to a second heat treatment in an oxygen atmosphere to obtain a positive electrode substrate coated with a rare earth oxide functional coating. The molar ratio of Gd2O3 to the positive electrode material is 0.03:1, the heat treatment temperature is 700°C, the time is 10 hours, and the flow rate of the oxygen atmosphere is 0.5m 3 / h.

[0150] (f) The composite positive electrode material coated in step (e) is sieved through a sieve having a mesh size of 300 to obtain a final positive electrode active material.

[0151] Application Example 4

[0152] The difference from Application Example 1 is that the double-layered positive electrode material precursor is replaced by the double-layered positive electrode material precursor of Example 2.

[0153] Application Example 5

[0154] The difference from Application Example 1 is that the double-layered positive electrode material precursor is replaced by the double-layered positive electrode material precursor of Example 3.

[0155] Application Example 6

[0156] The difference from Application Example 1 is that the double-layer structured positive electrode material precursor is replaced by the double-layer structured positive electrode material precursor of Example 4.

[0157] Application Example 7

[0158] The difference from Application Example 1 is that the double-layered positive electrode material precursor is replaced by the double-layered positive electrode material precursor of Example 5.

[0159] Application Example 8

[0160] The difference from Application Example 1 is that the double-layered positive electrode material precursor is replaced by the double-layered positive electrode material precursor of Example 6.

[0161] Application Example 9

[0162] The difference from Application Example 1 is that the double-layered positive electrode material precursor is replaced by the double-layered positive electrode material precursor of Example 7.

[0163] Application Example 10

[0164] The difference from Application Example 1 is that the double-layer structured positive electrode material precursor is replaced by the double-layer structured positive electrode material precursor of Example 8.

[0165] Application Example 11

[0166] The difference from Application Example 1 is that the double-layered positive electrode material precursor is replaced by the double-layered positive electrode material precursor of Example 9.

[0167] Application Example 1

[0168] The difference from Application Example 1 is that the positive electrode material precursor with a double-layer structure is replaced by the positive electrode material precursor of Comparative Example 1.

[0169] Application Example 2

[0170] The difference from Application Example 1 is that the positive electrode material precursor with a double-layer structure is replaced by the positive electrode material precursor of Comparative Example 2.

[0171] Application Example 3

[0172] The difference from Application Example 1 is that the positive electrode material precursor with a double-layer structure is replaced by the positive electrode material precursor of Comparative Example 3.

[0173] test:

[0174] The composite positive electrode material obtained in application examples 1-11 and application control examples 1-3 was mixed with the conductive agent Super P and the binder PVDF in a mass ratio of 90:6:4, and an appropriate amount of 1-methyl-2-pyrrolidone NMP was added. The slurry was prepared by ball milling with zirconium oxide beads for 1 hour, and then evenly coated on the aluminum sheet, vacuum dried, and rolled to form a positive electrode sheet. Graphite was used as the negative electrode active material and was mixed with the conductive agent Super P and the binder SBR in a mass ratio of 95:3:2, and water was added to form a homogenous slurry, and then evenly coated on the copper foil, vacuum dried, and rolled to form a negative electrode sheet. The above-mentioned positive electrode sheet, negative electrode sheet, separator and electrolyte were assembled into a single-chip soft-pack battery.

[0175] The battery performance test was performed using a blue power test system (charge and discharge voltage was 2.75-4.25V, temperature condition was 45°C). The battery performance test results are shown in Table 1.

[0176] Table 1 Rate performance test results

[0177]

[0178]

[0179] analyze:

[0180] By comparing Application Example 1 with Application Examples 6-7, it can be seen that Application Examples 6-7 use the precursor prepared in Example 4-5. Since the fluoride ion concentration in the system during the co-precipitation reaction in step (c) is too low, the primary particles of the material are not sufficiently refined, the density is insufficient, the structural stability is deteriorated, and the electrochemical performance is reduced.

[0181] By comparing Application Example 1 with Application Examples 8-9, it can be seen that Application Examples 8-9 use the precursor prepared in Examples 6-7. Since the fluoride ion concentration in the reaction system during the co-precipitation reaction in step (d) is too high, the reaction process is redundant and impurities may be formed, thereby reducing the electrochemical properties of the material.

[0182] By comparing Application Example 1 with Application Examples 10-11, it can be seen that Application Examples 10-11 use the precursor prepared in Examples 8-9, and the flow rate relationship between the mixed metal salt solution B and the mixed metal salt solution A and the flow rate difference between the two will affect the structure and composition of the positive electrode precursor. By preferably having an input flow rate of the mixed metal salt solution B greater than the input flow rate of the mixed metal salt solution A, and the flow rate difference between the input flow rate of the mixed metal salt solution B and the input flow rate of the mixed metal salt solution A is 50L / h to 300L / h, better rate performance can be obtained.

[0183] By comparing Application Example 1 with Application Control Example 1, it can be seen that the composition of the core and the shell are interchanged, the rate performance is deteriorated, and the Co element is in the core, so the rate performance is deteriorated.

[0184] By comparing Application Example 1 with Application Control Example 2, it can be seen that the inner core is not doped with fluorine and nitrogen, the primary particles of the inner core are not densely doped, the structural stability is deteriorated, and the electrochemical performance of the material is deteriorated.

[0185] By comparing Application Example 1 with Application Control Example 3, it can be seen that the outer core is not doped with fluorine and nitrogen, the primary particles of the outer core are not refined by doping, are not dense enough, the structural stability is deteriorated, and the electrochemical properties of the material are deteriorated.

[0186] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A positive electrode active material, It is characterized in that The positive electrode active material is prepared by using a positive electrode material precursor, and the positive electrode active material includes nickel-iron-manganese-aluminum oxide and nickel-cobalt-aluminum oxide, wherein the nickel-iron-manganese-aluminum oxide is doped with fluorine and nitrogen, and the nickel-cobalt-aluminum oxide is doped with fluorine and nitrogen; The positive electrode material precursor comprises a core and a shell coated on the surface of the core, wherein the core is fluorine- and nitrogen-doped nickel-iron-manganese-aluminum hydroxide, and the chemical formula of the core is Ni x1 Fe y1 Mn z1 Al h1 (OH) 2-a1-b1 F a1 N b1 , 0.1≤x1≤0.9, 0.05≤y1≤0.3, 0.05≤z1≤0.3, 0.05≤h1≤0.3, x1+y1+z1+h1=1, 0.01≤a1≤0.2, 0.01≤b1≤0.2, the shell is fluorine and nitrogen doped nickel cobalt aluminum hydroxide, the chemical formula of the shell is Ni x3 Co y3 Al z3 (OH) 2-a2-b2 F a2 N b2 , 0.1≤x3≤0.8, 0.1≤y3≤0.8, 0.1≤z3≤0.8, x3+y3+z3=1, 0.01≤a2≤0.2, 0.01≤b2≤0.2; The outer surface of the nickel-cobalt-aluminum oxide is provided with a rare earth oxide functional coating; The positive electrode active material is prepared by the following method, which comprises: After mixing the cathode material precursor and the lithium source, a first heat treatment is performed to obtain the cathode active material; After mixing the positive electrode active material and the rare earth oxide, a second heat treatment is performed to obtain the positive electrode active material with a coating layer; The molar ratio of the rare earth oxide to the positive electrode active material is (0.01-0.1):

1.

2. The positive electrode active material according to claim 1, It is characterized in that The particle size D50 of the inner core is 3 μm to 6 μm.

3. The positive electrode active material according to claim 1, It is characterized in that The particle size D50 of the positive electrode material precursor is 10 μm to 15 μm.

4. A method for preparing a cathode material precursor according to any one of claims 1 to 3, It is characterized in that The method comprises the following steps: (a) Solution preparation: A mixed metal salt solution A is prepared by using nickel salt, iron salt, manganese salt and aluminum salt; A mixed metal salt solution B is prepared by using nickel salt, cobalt salt and aluminum salt; preparing a precipitant solution, a complexing agent solution, a fluorine source solution and a nitrogen source solution; (b) Coprecipitation reaction: A mixed metal salt solution A, a precipitant solution, a complexing agent solution, a fluorine source solution and a nitrogen source solution are introduced into a reaction container containing a base liquid to carry out a first coprecipitation reaction. After obtaining an inner core of a preset particle size, the mixed metal salt solution A is replaced with a mixed metal salt solution B, and a second coprecipitation reaction is continued to obtain the positive electrode material precursor.

5. The method according to claim 4, It is characterized in that The concentration of the mixed metal salt solution A in step (a) is 0.5 mol / L to 3 mol / L.

6. The method according to claim 4, It is characterized in that The concentration of the mixed metal salt solution B in step (a) is 0.7 mol / L to 4.0 mol / L.

7. The method according to claim 4, It is characterized in that The fluorine source in the fluorine source solution in step (a) comprises at least one of sodium fluoride, potassium fluoride and magnesium fluoride.

8. The method according to claim 4, It is characterized in that The nitrogen source in the nitrogen source solution in step (a) comprises at least one of sodium nitride, potassium nitride and magnesium nitride.

9. The method according to claim 4, It is characterized in that During the entire reaction process of step (b), the reaction temperature is in the range of 50°C to 70°C, the pH value of the reaction system is in the range of 11 to 13, and the reaction is accompanied by stirring at a stirring speed in the range of 200rpm to 800rpm.

10. The method according to claim 4, It is characterized in that During the entire reaction process of step (b), the concentration of the complexing agent in the reaction system is 4.0 mol / L to 15.0 mol / L.

11. The method according to claim 4, It is characterized in that During the entire reaction process of step (b), the concentration of fluoride ions in the reaction system is in the range of 0.5 mmol / L to 2.0 mmol / L, and the concentration of nitrogen ions is in the range of 0.5 mmol / L to 2.0 mmol / L.

12. The method according to claim 4, It is characterized in that In step (b), the flow rate of the mixed metal salt solution B is greater than the flow rate of the mixed metal salt solution A.

13. The method according to claim 4, It is characterized in that The flow rate difference between the inlet flow rate of the mixed metal salt solution B and the inlet flow rate of the mixed metal salt solution A is 50 L / h to 300 L / h.

14. The method according to claim 4, It is characterized in that The inlet flow rate of the mixed metal salt solution A is 60 L / h to 300 L / h.

15. The method according to claim 4, It is characterized in that The flow rate of the mixed metal salt solution B is 200L / h~600L / h.

16. The method according to claim 4, It is characterized in that The method further comprises the step of introducing a protective gas into the reaction container, wherein the introduction flow rate of the protective gas is 10 L / min to 500 L / min.

17. A method for preparing a positive electrode active material according to any one of claims 1 to 3, It is characterized in that The method comprises the following steps: mixing a positive electrode material precursor and a lithium source, and then subjecting the mixture to a first heat treatment to obtain a positive electrode active material.

18. The method according to claim 17, It is characterized in that The temperature of the first heat treatment is 600°C to 900°C.

19. The method according to claim 17, It is characterized in that The first heat treatment time is 6h~20h.

20. The method according to claim 17, It is characterized in that The first heat treatment is performed in an oxygen atmosphere.

21. The method according to claim 17, It is characterized in that In the first heat treatment, the gas flow rate of the oxygen atmosphere is 0.2m 3 / h~2.0m 3 / h.

22. The method according to claim 17, It is characterized in that The first heat treatment is carried out by microwave heating.

23. The method according to claim 17, It is characterized in that The method also includes the step of coating the positive electrode active material, specifically including: mixing the positive electrode material and the rare earth oxide, and performing a second heat treatment to obtain a positive electrode material with a coating layer; the molar ratio of the rare earth oxide to the positive electrode active material is (0.01~0.1):

1.

24. The method according to claim 23, It is characterized in that The temperature of the second heat treatment is 600°C to 900°C.

25. The method according to claim 23, It is characterized in that The second heat treatment time is 5h~20h.

26. The method according to claim 23, It is characterized in that The second heat treatment is performed in an oxygen atmosphere.

27. The method according to claim 23, It is characterized in that In the second heat treatment, the gas flow rate of the oxygen atmosphere is 0.1m 3 / h~2.0m 3 / h.

28. The method according to claim 23, It is characterized in that The positive electrode material is preliminarily washed before being mixed with the rare earth oxide.

29. The method according to claim 28, It is characterized in that The detergent used in the washing process is deionized water.

30. The method according to claim 28, It is characterized in that During the washing process, the mass ratio of deionized water to the positive electrode material is (1-2):1, and the washing time is 5 min-30 min.

31. The method according to claim 28, It is characterized in that The washing process is followed by a drying process.

32. The method according to claim 31, It is characterized in that The drying process is: drying in a rotary vacuum drying furnace, and the rotation speed of the rotary vacuum drying furnace is 60r / min~200r / min.

33. A lithium ion battery, It is characterized in that The positive electrode of the lithium-ion battery comprises the positive electrode active material according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Preparation method of cathode material lithium nickel manganese aluminum oxide of lithium ion battery

    CN103117387A

  • Method for preparing modified lithium nickel manganese oxide which is anode material of lithium ion battery

    CN105322151A

  • Carbon material with nitrogen, fluorine and transition metal co-doped graphene structure and one-step carbonization preparation method thereof

    CN110148762A

  • Positive electrode material and preparation method thereof, lithium ion battery and vehicle

    CN110707296A

  • NCMA positive electrode material with core-shell structure and preparation method of NCMA positive electrode material