Carbon nanotube modified polypropylene composite material and preparation method thereof, and injection molded product

By using the combined design of segmented shear elements and toothed disks in the twin-screw extruder, the problem of poor dispersion of carbon nanotubes in polypropylene composite materials was solved, and the surface of the part was pit-free, with high conductive performance and Excellent mechanical properties.

CN116239840BActive Publication Date: 2024-10-22SHENZHEN XIWAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310156322.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-10-22
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The poor dispersion of carbon nanotubes in carbon nanotube-modified polypropylene composite materials leads to the formation of pitted particles on the surface of injection molded parts, affecting the appearance and subsequent performance of the parts.

Method used

A twin-screw extruder is used for extrusion and granulation, and the agglomeration of carbon nanotubes is opened through the combination of step-by-step enhanced shear elements in the melting and plasticizing section and the arrangement and combination of shear blades and toothed discs in the mixing and homogenizing section. body to achieve uniform dispersion in polypropylene resin, avoid agglomeration of carbon nanotubes, and control the temperature of each section of the extruder to 220 to 250°C to prevent carbonization.

Benefits of technology

It achieves uniform dispersion of carbon nanotubes in polypropylene composite materials, eliminates pitting particles on the surface of the parts, improves the conductivity, surface flatness and mechanical mechanical properties of the material, and is suitable for semiconductor and electronic packaging fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116239840B_ABST
    Figure CN116239840B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of material technology, and in particular, relates to a carbon nanotube-modified polypropylene composite material and a preparation method thereof, as well as an injection molded part. The preparation method comprises the steps of obtaining a raw material component including 50 to 100 parts of polypropylene resin, 0.1 to 10 parts of conductive agent, 0 to 10 parts of toughening agent, 0 to 30 parts of filler, 0 to 2 parts of pigment and 0 to 2 parts of auxiliary agent; the conductive agent comprises carbon nanotubes; after the raw material components are made into a mixed material, they are added to a twin-screw extruder for extrusion granulation to obtain a carbon nanotube-modified polypropylene composite material; wherein, the temperature of each section in the twin-screw extruder is 220 to 250°C, the melt plasticization section adopts a combination of shear elements reinforced in sections, and the mixing and homogenizing section adopts an arrangement and combination of shear blades and toothed discs. Through the specific design of the threaded element in the twin-screw extruder, the components are evenly distributed, and the composite material part has high conductivity, surface flatness and mechanical properties at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of material technology, and in particular relates to a carbon nanotube-modified polypropylene composite material and a preparation method thereof, as well as an injection molded part. Background Art

[0002] There are many types of antistatic materials on the market. Traditional conductive materials add conductive carbon black, which has poor conductivity and requires a large amount of addition. The fluidity becomes poor during processing. In addition, there is mold dust, which is easy to fall off during production and contaminate the carrier. Friction easily causes carbon powder to fall off, which is easy to pollute electronic components and even scrap them.

[0003] Polypropylene (PP), a semi-crystalline plastic, has the characteristics of low density and easy processing. The polypropylene composite material modified by carbon nanotubes has high conductivity and excellent fluidity, and is widely used in semiconductors, electronic packaging, transportation and other fields. However, due to the poor dispersibility of carbon nanotubes themselves, they are very easy to agglomerate during the modification process, resulting in the formation of pitted particles on the surface of the injection molded parts, affecting the appearance and subsequent performance of the parts. Summary of the invention

[0004] The purpose of the present application is to provide a carbon nanotube-modified polypropylene composite material and a preparation method thereof, as well as an injection molded part, aiming to solve to a certain extent the problem that the carbon nanotubes in the existing carbon nanotube-modified polypropylene composite material have poor dispersion, resulting in the formation of pitted particles on the surface of the injection molded part, affecting the appearance of the part and subsequent performance.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, the present application provides a method for preparing a carbon nanotube-modified polypropylene composite material, comprising the following steps:

[0007] Obtaining a raw material component including 50 to 100 parts of polypropylene resin, 0.1 to 10 parts of conductive agent, 0 to 10 parts of toughening agent, 0 to 30 parts of filler, 0 to 2 parts of pigment and 0 to 2 parts of auxiliary agent; wherein the conductive agent includes carbon nanotubes;

[0008] After the raw material components are made into a mixed material, they are added to a twin-screw extruder for extrusion granulation to obtain a carbon nanotube-modified polypropylene composite material; wherein the temperature of each section in the twin-screw extruder is 220-250° C., the melting and plasticizing section adopts a combination of shear elements that are reinforced section by section, and the mixing and homogenizing section adopts an arrangement and combination of shear plates and toothed disks.

[0009] In some possible implementations, the twin-screw extruder sequentially comprises a material conveying section, the melt plasticizing section, the mixing and homogenizing section, a vacuum exhaust section, and an extrusion pressure building section.

[0010] In some possible implementations, the temperature of each section in the twin-screw extruder is 220-250° C., and the screw speed is 300-600 rpm.

[0011] In some possible implementations, the screw combination order of the melt plasticization section is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56 and 44 / 22L.

[0012] In some possible implementations, the screw combination order of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56 and K90° / 45 / 56.

[0013] In some possible implementations, the screw combination sequence of the material conveying section is: 56 / 56, 96 / 96, 96 / 96, 96 / 48, 72 / 72, 64 / 64, 44 / 44 and 44 / 44.

[0014] In some possible implementations, the screw combination sequence of the vacuum exhaust section is: 44 / 22L, 72 / 72, 72 / 72, 72 / 72, 72 / 72 and 72 / 72.

[0015] In some possible implementations, the screw combinations of the extrusion pressure building section are in the following order: 64 / 64, 56 / 56, 44 / 44, 44 / 44 and 44 / 44.

[0016] In some possible implementations, the raw material components include 50 to 100 parts of polypropylene resin, 1 to 10 parts of conductive agent, 1 to 10 parts of toughening agent, 1 to 30 parts of filler, 0 to 2 parts of pigment and 1 to 2 parts of auxiliary agent; the conductive agent is carbon nanotubes.

[0017] In some possible implementations, the polypropylene resin is a composite product of a high-flow-rate polypropylene with a melt flow rate of 10 to 20 g / 10 min and a low-flow-rate polypropylene with a melt flow rate of 0.5 to 5 g / 10 min.

[0018] In some possible implementations, the density of the toughening agent is 0.80 to 0.90 g / cm3 , the melt flow rate is 0.1~2g / 10min.

[0019] In some possible implementations, the filler is selected from at least one of talc, barium sulfate, calcium carbonate, and wollastonite.

[0020] In some possible implementations, the pigment is selected from at least one of carbon black and black species.

[0021] In some possible implementations, the auxiliary agent is selected from at least one of a compatibilizer and a lubricant.

[0022] In some possible implementations, the carbon nanotubes include at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes.

[0023] In some possible implementations, the carbon nanotubes include at least one of array carbon nanotubes, acidified carbon nanotubes, and sulfide carbon nanotubes.

[0024] In some possible implementations, the mass ratio of the high flow rate polypropylene to the low flow rate polypropylene is (5-10):1.

[0025] In some possible implementations, the carbon nanotubes are selected from chiral carbon nanotubes with a diameter of 2 to 20 nm, a length of 0.1 to 100 μm, an aspect ratio of (8000 to 15000): 1, and a specific surface area of ​​200 to 350 m 2 / g of multi-walled carbon nanotubes.

[0026] In some possible implementations, the toughening agent is selected from at least one of vinyl elastomers, propylene elastomers, ethylene propylene diene monomer rubber, acrylonitrile-styrene-butadiene copolymers, and hydrogenated acrylonitrile-styrene-butadiene elastomers.

[0027] In a second aspect, the present application provides a carbon nanotube-modified polypropylene composite material, characterized in that the polypropylene composite material is prepared according to the above method.

[0028] In a third aspect, the present application provides an injection-molded part, wherein the injection-molded part is made of the above-mentioned carbon nanotube-modified polypropylene composite material.

[0029] The preparation method of the carbon nanotube modified polypropylene composite material provided in the first aspect of the present application is to make the raw material components of the formula into a mixed material, and then use a twin-screw extruder with a specially designed screw combination to extrude and granulate. Among them, the melt plasticization section adopts a combination of shear elements that are reinforced section by section, and the agglomerates of carbon nanotubes are opened through strong shearing action; the mixing and homogenization section adopts an arrangement and combination of shearing pieces and toothed discs, which simultaneously play the role of shearing and dispersing uniformly. Make the carbon nanotube powder disperse more evenly in the polypropylene resin matrix, solve the problem of uneven dispersion of carbon nanotubes in polypropylene resin causing pitting particles on the surface of the product, and improve the appearance and subsequent use performance of the carbon nanotube modified polypropylene composite product. In addition, the temperature of each section in the twin-screw extruder is controlled to be 220-250°C to avoid the serious carbonization of the base resin in the screw barrel, which causes the problem of serious pitting particles on the surface of the material. The prepared carbon nanotube modified polypropylene composite material has the characteristics of high conductivity, surface flatness, mechanical mechanics, and easy processing, and can be used in the fields of wafer mold box and semiconductor loading.

[0030] The carbon nanotube-modified polypropylene composite material provided in the second aspect of the present application is prepared according to the above method, and each raw material component is evenly distributed in the composite material, especially the carbon nanotube conductive agent is not agglomerated, so that the surface of the injection-molded part of the carbon nanotube-modified polypropylene composite material is free of pits, and at the same time has high conductivity, surface flatness, mechanical properties, and easy processing.

[0031] The injection molded part provided in the third aspect of the present application is made of the above-mentioned carbon nanotube-modified polypropylene composite material, has no pitting on the surface, has high flatness, and has high electrical conductivity, mechanical properties and other properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0033] Figure 1 It is a schematic flow chart of a method for preparing a carbon nanotube-modified polypropylene composite material provided in an embodiment of the present application. DETAILED DESCRIPTION

[0034] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0035] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0036] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0037] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0038] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0039] The weight of the relevant components mentioned in the embodiments of the present specification can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components in the embodiments of the present specification is proportionally enlarged or reduced, it is within the scope disclosed in the embodiments of the present specification. Specifically, the mass in the embodiments of the present specification can be μg, mg, g, kg and other mass units known in the chemical industry.

[0040] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0041] As attached Figure 1As shown, the first aspect of the embodiment of the present application provides a method for preparing a carbon nanotube-modified polypropylene composite material, comprising the following steps:

[0042] S10. Obtaining a raw material component comprising 50 to 100 parts of a polypropylene resin, 0.1 to 10 parts of a conductive agent, 0 to 10 parts of a toughening agent, 0 to 30 parts of a filler, 0 to 2 parts of a pigment, and 0 to 2 parts of an additive; wherein the conductive agent comprises carbon nanotubes;

[0043] S20. After the raw material components are made into a mixed material, they are added to a twin-screw extruder for extrusion granulation to obtain a carbon nanotube-modified polypropylene composite material; wherein the temperature of each section in the twin-screw extruder is 220-250°C, the melt plasticization section adopts a combination of shear elements that are reinforced in stages, and the mixing and homogenization section adopts an arrangement and combination of shear plates and toothed disks.

[0044] The preparation method of the carbon nanotube modified polypropylene composite material provided in the first aspect of the embodiment of the present application is to make the raw material components of the formula into a mixed material, and then use a twin-screw extruder with a specially designed screw combination to extrude and granulate. Among them, the melt plasticization section adopts a combination of shear elements that are reinforced section by section, and the agglomerates of carbon nanotubes are opened through strong shearing action; the mixing and homogenization section adopts an arrangement and combination of shearing pieces and toothed discs, which simultaneously play the role of shearing and dispersing uniformly. Make the carbon nanotube powder disperse more evenly in the polypropylene resin matrix, solve the problem of uneven dispersion of carbon nanotubes in polypropylene resin causing pitting particles on the surface of the product, and improve the appearance and subsequent use performance of the carbon nanotube modified polypropylene composite product. In addition, the temperature of each section in the twin-screw extruder is controlled to be 220-250°C to avoid serious carbonization of the base resin in the screw barrel, which causes serious pitting particles on the surface of the material. The prepared carbon nanotube modified polypropylene composite material has the characteristics of high conductivity, surface flatness, mechanical mechanics, and easy processing, and can be used in the fields of wafer mold box and semiconductor loading.

[0045] In some possible implementations, in the above step S10, the raw material components of the carbon nanotube-modified polypropylene composite material include 50 to 100 parts of polypropylene resin, 0.1 to 10 parts of conductive agent, 0 to 10 parts of toughening agent, 0 to 30 parts of filler, 0 to 2 parts of pigment and 0 to 2 parts of auxiliary agent; wherein the conductive agent includes carbon nanotubes to improve the conductivity of the composite material; the polypropylene resin as the base resin has the characteristics of low density and easy processing; the toughening agent can improve the toughness of the composite material; the filler can improve the mechanical properties of the composite material; the pigment can give the composite material different colors to meet different application requirements; the auxiliary agent can improve the processing properties such as fluidity of the composite material.

[0046] In some possible implementations, the raw material components include 50-100 parts of polypropylene resin, 1-10 parts of conductive agent, 1-10 parts of toughening agent, 1-30 parts of filler, 0-2 parts of pigment and 1-2 parts of auxiliary agent; the conductive agent is carbon nanotube. In this case, the raw material component ratio is more conducive to improving the conductivity, mechanical properties, processability and other comprehensive properties of the carbon nanotube-modified polypropylene composite material.

[0047] In some possible implementations, the polypropylene resin is a compound product of a high-flow rate polypropylene with a melt flow rate (MFR) of 10 to 20 g / 10 min and a low-flow rate polypropylene with a melt flow rate (MFR) of 0.5 to 5 g / 10 min. The test conditions of the melt flow rate are 230°C × 2.16 kg. The embodiment of the present application uses a compound of high-flow rate polypropylene and low-flow rate polypropylene to improve the toughness of the composite material without affecting the processing performance of the composite material.

[0048] In some possible implementations, the mass ratio of high flow rate polypropylene to low flow rate polypropylene is (5-10):1; under this ratio, the toughness of the composite material can be better improved. In some specific embodiments, the mass ratio of high flow rate polypropylene to low flow rate polypropylene can be 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc.

[0049] In some possible implementations, the density of the toughening agent is 0.80 to 0.90 g / cm 3 , the melt flow rate is 0.1 to 2 g / 10 min. The test conditions of the melt flow rate are 190°C × 2.16 kg. In some possible implementations, the toughening agent is selected from at least one of vinyl elastomers, propylene elastomers, EPDM rubber, acrylonitrile-styrene-butadiene copolymers, and hydrogenated acrylonitrile-styrene-butadiene elastomers. These toughening agents used in the above embodiments of the present application can effectively reduce the brittleness of carbon nanotube-modified polypropylene composites and improve the impact resistance of carbon nanotube-modified polypropylene composites.

[0050] In some possible implementations, the filler is selected from at least one of talc, barium sulfate, calcium carbonate, and wollastonite; these fillers can reduce the shrinkage rate of carbon nanotube-modified polypropylene composite parts, improve the dimensional stability, surface finish, smoothness, and matte or matte properties of the products; improve the wear resistance of the products, and improve electrical conductivity, thermal conductivity, impact strength, and compression strength.

[0051] In some possible implementations, the pigment is selected from at least one of carbon black and black species; it not only provides color decoration for the carbon nanotube-modified polypropylene composite material, but also provides more improvements in physical and chemical properties for the carbon nanotube-modified polypropylene composite material, such as hiding power, light resistance, weather resistance, temperature resistance, chemical resistance, gloss and mechanical strength.

[0052] In some possible implementations, the additive is selected from at least one of a compatibilizer and a lubricant; wherein the compatibilizer can increase the compatibility of the raw material components, increase the adhesion between the raw material components, and form a stable structure. The function of the lubricant is to reduce the friction between the macromolecules of the polypropylene resin, improve the fluidity of the polymer composite material, reduce the friction between the polymer and the processing machinery, avoid adhesion between them, and reduce the surface roughness of the product.

[0053] In some possible implementations, the carbon nanotubes include at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes. In some possible implementations, the carbon nanotubes include at least one of array carbon nanotubes, acidified carbon nanotubes, and sulfide carbon nanotubes. These types of carbon nanotubes used in the embodiments of the present application all have excellent electrical conductivity, among which multi-walled carbon nanotubes, array carbon nanotubes, acidified carbon nanotubes, sulfide carbon nanotubes and other carbon nanotubes have relatively good dispersion properties. Considering the cost and mass production, multi-walled carbon nanotubes are preferred.

[0054] In some possible implementations, the conductive agent includes multi-walled carbon nanotubes, the multi-walled carbon nanotubes have a tube diameter of 2 to 20 nm, a length of 0.1 to 100 μm, an aspect ratio of (8000 to 15000): 1, and a specific surface area of ​​200 to 350 m 2 / g, and has chirality. The larger the aspect ratio and the larger the specific surface area of ​​the carbon nanotubes, the better the conductivity, but at the same time, the difficulty of dispersion is high. The carbon nanotubes with this physical and chemical parameters have both excellent dispersion and conductivity. In some specific embodiments, the diameter of the multi-walled carbon nanotubes can be 2-5nm, 5-10nm, 10-15nm, 15-20nm, etc., and the length can be 0.1-1μm, 1-2μm, 2-10μm, 10-30μm, 30-50μm, 50-80μm, 80-100μm, etc.; the aspect ratio can be (8000-9000): 1, (9000-10000): 1, (10000-12000): 1, (11000-15000): 1, etc.; the specific surface area can be 200-250m 2 / g, 250~300m 2 / g, 300~350m 2 / g, etc.

[0055] In some possible implementations, in the above step S20, a high-speed mixer is used to prepare a mixed material from the raw material components. Specifically, the mixing conditions include: a mixing temperature of 25 to 60° C., a rotation speed of 120 to 600 rpm, and a mixing time of 3 to 6 minutes, so that the raw material components are fully mixed to obtain a mixed material.

[0056] In some possible implementations, the twin-screw extruder includes a material conveying section, a melt-plasticizing section, a mixing and homogenizing section, a vacuum exhaust section, and an extrusion pressure building section in sequence. After the mixed material is added to the twin-screw extruder, it passes through the material conveying section, the melt-plasticizing section, the mixing and homogenizing section, the vacuum exhaust section, and the extrusion pressure building section in sequence to obtain an extruded granulated carbon nanotube-modified polypropylene composite material.

[0057] In some possible implementations, the temperature of each section in the twin-screw extruder is 220-250°C, and the screw speed is 300-600rpm. Under this temperature and speed condition, it is conducive to extrusion and granulation of the mixed material to obtain a carbon nanotube-modified polypropylene composite material. If the temperature or speed is too low, it is not conducive to uniform melting and mixing of the materials; if the temperature or speed is too high, it will cause the raw material components to be carbonized in the barrel, affecting the performance of the composite material.

[0058] In some possible implementations, the screw combination sequence of the melt plasticization section is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56 and 44 / 22L. In this case, the melt plasticization section adopts the step-by-step enhanced shear element combination of this specific sequence, and through the strong shearing action, the agglomerates of carbon nanotubes are opened, so that the carbon nanotubes can be evenly distributed in the base resin, and the formation of pitting on the surface of the composite material product is avoided.

[0059] In some possible implementations, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56 and K90° / 45 / 56. In this case, the mixing and homogenizing section adopts the arrangement and combination of the shearing blades and C18 toothed discs of this characteristic sequence, which plays the role of shearing and dispersing uniformly, so that the carbon nanotube powder is more evenly dispersed in the resin matrix, and the problem of particle pitting on the surface of the carbon nanotube-modified polypropylene composite material is solved.

[0060] In some possible implementations, the screw combination sequence of the material conveying section is: 56 / 56, 96 / 96, 96 / 96, 96 / 48, 72 / 72, 64 / 64, 44 / 44 and 44 / 44.

[0061] In some possible implementations, the screw combinations of the vacuum exhaust section are in the following order: 44 / 22L, 72 / 72, 72 / 72, 72 / 72, 72 / 72, and 72 / 72.

[0062] In some possible implementations, the screw combinations in the extrusion pressure building section are in the following order: 64 / 64, 56 / 56, 44 / 44, 44 / 44 and 44 / 44.

[0063] In the above embodiments of the present application, the threaded elements in the screw assembly of the twin-screw extruder are divided into conveying elements, shearing elements and special elements (such as stretching elements, dispersing element toothed discs, transition pieces, etc.). Among them, the threaded element representation method is as follows: the conveying element is composed of a lead and a length, and is divided into forward and reverse directions. The forward direction is represented by two numbers, and the reverse direction is represented by two numbers followed by an "L"; such as 56 / 56, the first "56" represents the lead (that is, the axial length of the material around the thread), and the second "56" represents the length of the threaded element (that is, the axial length of the element). Commonly used elements of the conveying block are 128 / 128, 96 / 96, 72 / 72, 64 / 64, 56 / 56, 44 / 44, 48 / 48, 32 / 32, 22 / 22, 96 / 48, 72 / 36, 44 / 22L, 22 / 11L. The shear element is kneaded together by multiple shear sheets, with 4 to 7 sheets and different thicknesses. Different kneading types are selected according to different needs. The thicker the shear sheet, the stronger the distribution ability, and the thinner the shear sheet, the stronger the dispersion ability; the larger the angle between the shear sheets, the stronger the shear ability, and it is also divided into positive and negative. The expression method is as follows: K angle / number of sheets / element length, such as reverse expression as K angle / number of sheets / element length L. Example of shear block model: K90° / 5 / 56L, 90 refers to the kneading angle of the single sheet is 90 degrees, 5 refers to the number of sheets, 56 refers to the length, and L refers to the left. Special shear elements include toothed discs and stretching blocks. The toothed disk mainly plays a dispersing role and is usually used in the homogenizing section at the rear end of the screw. It is expressed as C thickness, such as C18, which refers to a toothed disk with a thickness of 18mm. The stretching block also plays a dispersing and distributing role and is usually used in the homogenizing section at the rear end of the screw. It is expressed as lead / length L, such as 78 / 78L, which means a reverse stretching element with a lead of 78 and an element length of 78.

[0064] The twin-screw extruder used in the present application comprises a feed material conveying section, a melt plasticizing section, a mixing and homogenizing section, a vacuum exhaust section and an extrusion pressure building section, wherein the screw combination of the melt plasticizing section and the mixing and homogenizing section has the greatest influence on the surface pitting particles of the carbon nanotube-modified polypropylene composite material and plays a decisive role. By using a combination of shear elements that are reinforced section by section in the melt plasticizing section of the extruder screw and a strong dispersion element combination design in the mixing and homogenizing section, the mixed material is first subjected to strong shearing to obtain sufficient melt plasticization after entering the extruder, and then is fully mixed and dispersed by the strong dispersion element at the rear end. In this way, the resin melt and the filling powders such as carbon nanotubes in the entire melt system are fully dispersed and uniform, without agglomeration, thereby improving the surface flatness and smoothness and reducing the pitting particles on the surface of the product.

[0065] A second aspect of an embodiment of the present application provides a carbon nanotube-modified polypropylene composite material, which is prepared according to the above method.

[0066] The carbon nanotube-modified polypropylene composite material provided in the second aspect of the embodiment of the present application is prepared according to the above method, and each raw material component is evenly distributed in the composite material, especially the carbon nanotube conductive agent is not agglomerated, so that the surface of the injection-molded part of the carbon nanotube-modified polypropylene composite material is free of pits, and at the same time has high conductivity, surface flatness, mechanical properties, and easy processing.

[0067] A third aspect of an embodiment of the present application provides an injection-molded part, which is made of the above-mentioned carbon nanotube-modified polypropylene composite material.

[0068] The injection molded part provided in the third aspect of the embodiment of the present application is made of the above-mentioned carbon nanotube-modified polypropylene composite material, has no pitting on the surface, has high flatness, and has high electrical conductivity, mechanical properties and other properties.

[0069] In some possible implementations, the injection molded parts include wafer mold boxes, semiconductor packaging materials, etc.

[0070] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, as well as to demonstrate the significant improvement in performance of the carbon nanotube-modified polypropylene composite material and its preparation method in the embodiments of the present application, the above technical scheme is illustrated by multiple embodiments below.

[0071] Example 1

[0072] A carbon nanotube-modified polypropylene composite material, the raw material components of which are shown in the material ratios in Table 1 below.

[0073] The preparation steps include:

[0074] After the raw material components are evenly mixed, they are added into a twin-screw extruder, and screw combination ① is selected for melt mixing, that is, the screw combination sequence of the melt plasticizing section of the extruder is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56, 44 / 22L, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56. The temperature of each section of the extruder is 230°C, the screw speed is 400 rpm, and extrusion granulation is carried out to obtain a carbon nanotube modified polypropylene composite material.

[0075] Example 2

[0076] A carbon nanotube-modified polypropylene composite material, the raw material components of which are shown in the material ratios in Table 1 below.

[0077] The preparation steps include:

[0078] After the raw material components are evenly mixed, they are added into a twin-screw extruder, and screw combination ① is selected for melt mixing, that is, the screw combination sequence of the melt plasticizing section of the extruder is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56, 44 / 22L, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56. The temperature of each section of the extruder is 230°C, the screw speed is 400 rpm, and extrusion granulation is carried out to obtain a carbon nanotube modified polypropylene composite material.

[0079] Example 3

[0080] A carbon nanotube-modified polypropylene composite material, the raw material components of which are shown in the material ratios in Table 1 below.

[0081] The preparation steps include:

[0082] After the raw material components are evenly mixed, they are added into a twin-screw extruder, and screw combination ① is selected for melt mixing, that is, the screw combination sequence of the melt plasticizing section of the extruder is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56, 44 / 22L, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56. The temperature of each section of the extruder is 230°C, the screw speed is 400 rpm, and extrusion granulation is carried out to obtain a carbon nanotube modified polypropylene composite material.

[0083] Comparative Example 1

[0084] A carbon nanotube-modified polypropylene composite material, the raw material components of which are shown in the material ratios in Table 1 below.

[0085] The preparation steps include:

[0086] After the raw material components are evenly mixed, they are added to a twin-screw extruder, and screw combination ② is selected for melt mixing, that is, the screw combination sequence of the melt plasticizing section of the extruder is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 5 6. K60° / 4 / 44, K90° / 45 / 56, 44 / 22L, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 56 / 56, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 56 / 56, 44 / 44, K60° / 4 / 56, K90° / 45 / 56. The temperature of each section of the extruder is 230°C, the screw speed is 400 rpm, and extrusion granulation is carried out to obtain a carbon nanotube modified polypropylene composite material.

[0087] Comparative Example 2

[0088] A carbon nanotube-modified polypropylene composite material, the raw material components of which are shown in the material ratios in Table 1 below.

[0089] The preparation steps include:

[0090] After the raw material components are evenly mixed, they are added into a twin-screw extruder, and screw combination ③ is selected for melt mixing, that is, the screw combination sequence of the melt plasticizing section of the extruder is K45° / 5 / 56, K60° / 4 / 44, 56 / 56, 44 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 56 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44 , 44 / 22L, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56. The temperature of each section of the extruder is 230°C, the screw speed is 400 rpm, and extrusion granulation is carried out to obtain a carbon nanotube modified polypropylene composite material.

[0091] Comparative Example 3

[0092] A carbon nanotube-modified polypropylene composite material, the raw material components of which are shown in the material ratios in Table 1 below.

[0093] The preparation steps include:

[0094] After the raw material components are evenly mixed, they are added into a twin-screw extruder, and screw combination ① is selected for melt mixing, that is, the screw combination sequence of the melt plasticizing section of the extruder is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56, 44 / 22L, the screw combination sequence of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56. The temperature of each section of the extruder is 260°C, the screw speed is 400 rpm, and extrusion granulation is carried out to obtain a carbon nanotube modified polypropylene composite material.

[0095] The formulas of the carbon nanotube-modified polypropylene composite materials of the above-mentioned embodiments and comparative examples are shown in Table 1 below:

[0096] Table 1

[0097] Item / Content Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 PP1 30.2 30.2 30.2 30.2 30.2 30.2 PP2 31 31 31 31 31 31 Toughening agent 6 6 6 6 6 6 Compatibilizer 0.5 0.5 0.5 0.5 0.5 0.5 Lubricants 0.3 0.3 0.3 0.3 0.3 0.3 talcum powder 19 19 19 19 19 19 pigment 1 1 1 1 1 1 CNT 4.5 5 5.5 4.5 4.5 4.5 Speed ​​rpm 400 400 400 400 400 400 Temperature ℃ 230 230 230 230 230 260 Screw combination Combination ① Combination ① Combination ① Combination ② Combination ③ Combination ①

[0098] Among them, the main material PP1 is a high-flow polypropylene resin, and the melt index is 10-20g / 10min at 230℃×2.16k; the main material PP2 is a low-flow polypropylene resin, and the melt index is 0.5-5g / 10min at 230℃×2.16kg. The toughening agent is commercially available POE with a density of 0.80-0.9g / cm 3 , the melt index is 0.1-2g / 10min at 190℃×2.16kg. The filler is talcum powder. The pigment is black. The lubricant is silicone powder TS-LS100, and the compatibilizer is model BIA.

[0099] Further, in order to verify the progress of the embodiments of the present application, the density, melt index, tensile strength, flexural strength, flexural modulus, impact strength, surface resistivity, and the effect of pitting particles on the surface of the carrier tape of the carbon nanotube-modified polypropylene composite material parts prepared in each embodiment and comparative example were tested respectively. The test results are shown in Table 2 below:

[0100] Table 2

[0101]

[0102] It can be seen from the test results in Table 2 above that compared with Example 1, the screw combinations used in Comparative Examples 1 and 2 are ② and ③ respectively, which cannot effectively eliminate the pitting particles on the surface of the carbon nanotube-modified polypropylene composite material, and the surface impedance is also up to standard, and other mechanical properties are also reduced. It shows that the screw combination ① of the embodiment of the present application can significantly eliminate the pitting particles on the surface of the polypropylene composite material, and the surface impedance is also up to standard. The screw combination ① is a combination of threaded elements with shear enhancement in the front melt plasticization section and a special dispersing element C18 toothed disk added to the rear homogenization section, so that the carbon nanotube powder can be fully dispersed in the resin matrix, and there is no pitting particle phenomenon on the surface of the product. However, in the screw combinations ② and ③ in the comparative examples, the melt plasticization section does not adopt a shear element combination that is enhanced step by step, and the mixing and homogenization section does not adopt a specific toothed disk dispersing element and shear element, resulting in the carbon nanotubes not being fully sheared and dispersed in the barrel, agglomeration occurs, and there are more pitting particles on the surface of the product.

[0103] Compared with Example 1, Comparative Example 3 shows that after the temperature is increased, the base resin is severely carbonized in the barrel, resulting in serious pitting particles on the surface of the material. Compared with Example 1, Examples 2 and 3 have different amounts of carbon nanotubes added. From the results, it can be seen that the greater the amount of carbon nanotubes added, the better the resistance impedance of the product, but the lower the melt index.

[0104] In addition, six groups of parallel experiments were conducted on Example 2 to test the process stability of the preparation method of the carbon nanotube-modified polypropylene composite material. The test results are shown in Table 3:

[0105] Table 3

[0106]

[0107] It can be seen from the test results in Table 3 above that the preparation method of the carbon nanotube-modified polypropylene composite material in the embodiment of the present application has high process stability. Six groups of parallel experiments were carried out using this process method. The surface pitting and particle effects of the prepared carbon nanotube-modified polypropylene composite materials were all OK and met the standards, and the surface resistivity also maintained stability.

[0108] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a carbon nanotube-modified polypropylene composite material, characterized in that: The following steps are involved: Obtain raw material components including 50-100 parts of polypropylene resin, 0.1-10 parts of conductive agent, 0-10 parts of toughening agent, 0-30 parts of filler, 0-2 parts of pigment and 0-2 parts of auxiliary agent; wherein the conductive agent includes chiral tubes with a diameter of 2-20 nm, a length of 0.1-100 μm, an aspect ratio of (8000-15000): 1, and a specific surface area of ​​200-350 m 2 / g of multi-walled carbon nanotubes; the polypropylene resin is a composite product of a high-flow rate polypropylene with a melt flow rate of 10 to 20 g / 10min and a low-flow rate polypropylene with a melt flow rate of 0.5 to 5 g / 10min in a mass ratio of (5 to 10):1; wherein the test conditions of the melt flow rate are 230°C×2.16kg; After the raw material components are made into a mixed material, the mixed material is added into a twin-screw extruder for extrusion granulation to obtain a carbon nanotube-modified polypropylene composite material; wherein the temperature of each section in the twin-screw extruder is 220-250° C., the melting and plasticizing section adopts a combination of shear elements reinforced in sections, and the mixing and homogenizing section adopts an arrangement and combination of shear plates and toothed discs; The screw combination order of the melt plasticization section is K30° / 7 / 64, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, 44 / 44, K60° / 4 / 44, K90° / 45 / 56, 44 / 44, K45° / 5 / 56, K60° / 4 / 44, K90° / 45 / 56 and 44 / 22L; the screw combination order of the mixing and homogenizing section is K45° / 5 / 56, K60° / 4 / 56, K90° / 45 / 56, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56, K90° / 45 / 56, K45° / 5 / 36L, 44 / 44, C18, C18, 44 / 44, K60° / 4 / 56 and K90° / 45 / 56; Among them, the conveying element is composed of lead and length, and there are positive and negative directions. The positive direction is represented by two numbers, and the reverse direction is represented by two numbers followed by an "L"; the shear element is represented by: K angle / number of pieces / element length, the toothed disc is represented by: C thickness; the stretching block is represented by: lead / length L.

2. The method for preparing the carbon nanotube-modified polypropylene composite material according to claim 1, characterized in that: The twin-screw extruder comprises a material conveying section, a melting and plasticizing section, a mixing and homogenizing section, a vacuum exhaust section and an extrusion pressure building section in sequence; And / or, the temperature of each section in the twin-screw extruder is 220-250° C., and the screw speed is 300-600 rpm.

3. The method for preparing the carbon nanotube-modified polypropylene composite material according to claim 2, characterized in that: The screw combination sequence of the material conveying section is: 56 / 56, 96 / 96, 96 / 96, 96 / 48, 72 / 72, 64 / 64, 44 / 44 and 44 / 44; And / or, the screw combination sequence of the vacuum exhaust section is: 44 / 22L, 72 / 72, 72 / 72, 72 / 72, 72 / 72 and 72 / 72; And / or, the screw combination sequence of the extrusion pressure building section is: 64 / 64, 56 / 56, 44 / 44, 44 / 44 and 44 / 44.

4. The method for preparing the carbon nanotube-modified polypropylene composite material according to claim 3, characterized in that: The raw material components include 50-100 parts of polypropylene resin, 1-10 parts of conductive agent, 1-10 parts of toughening agent, 1-30 parts of filler, 0-2 parts of pigment and 1-2 parts of auxiliary agent; the conductive agent is carbon nanotube.

5. The method for preparing the carbon nanotube-modified polypropylene composite material according to claim 4, characterized in that: The density of the toughening agent is 0.80-0.90 g / cm 3 , the melt flow rate is 0.1-2 g / 10 min; wherein, the test conditions of the melt flow rate are 190°C×2.16 kg; And / or, the filler is selected from at least one of talc, barium sulfate, calcium carbonate or wollastonite; And / or, the pigment is selected from carbon black; And / or, the auxiliary agent is selected from at least one of a compatibilizer or a lubricant; And / or, the carbon nanotubes include at least one of array carbon nanotubes, acidified carbon nanotubes or sulfide carbon nanotubes.

6. The method for preparing the carbon nanotube-modified polypropylene composite material according to claim 5, characterized in that: The toughening agent is selected from at least one of vinyl elastomer, propylene elastomer, acrylonitrile-styrene-butadiene copolymer, and hydrogenated acrylonitrile-styrene-butadiene elastomer.

7. A carbon nanotube-modified polypropylene composite material, characterized in that: The polypropylene composite material is prepared according to the method according to any one of claims 1 to 6.

8. An injection molded part, characterized in that: The injection molded part is made of the carbon nanotube-modified polypropylene composite material as claimed in claim 7.