Magnesium alloy titanium aluminum tungsten film treatment agent, preparation method and magnesium alloy surface treatment method
Through the preparation of magnesium alloy titanium aluminum tungsten film treatment agent, 98% sulfuric acid, 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol are used to form a stable titanium aluminum tungsten film, which solves the problem of magnesium alloy corrosion resistance The problems of insufficient and toxic vanadate contamination have been achieved, and the high corrosion resistance and environmental protection of magnesium alloys have been achieved.
Patent Information
- Application Number
- CN202211595254.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-13
AI Technical Summary
The existing phosphorus-free and chromium-free conversion coating treatment agents for magnesium alloys perform poorly in terms of corrosion resistance and contain toxic pentavalent vanadate, which pollutes the environment and harms human health.
The magnesium alloy titanium aluminum tungsten film treatment agent is used to form a titanium aluminum tungsten film with stable performance by formulating a suitable combination of 98% sulfuric acid, 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol. Avoid using 5-valent vanadate to improve the corrosion resistance and environmental protection of magnesium alloys.
The corrosion resistance and environmental protection of magnesium alloys are significantly improved. The magnesium alloys maintain good performance under continuous spraying of 5% sodium chloride neutral salt spray for more than 48 hours without black corrosion spots, meeting higher corrosion resistance requirements and avoiding environmental pollution and human health hazards.
Smart Images

Figure CN116240535B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, and in particular to a magnesium alloy titanium aluminum tungsten film treatment agent, a preparation method and a magnesium alloy surface treatment method. Background Art
[0002] As a widely used industrial material, magnesium alloy has attracted extensive attention from various industries such as aerospace, automobile, electronics, precision instruments, etc. due to its advantages of low density, light weight, good shock absorption, strong impact resistance, good electromagnetic shielding, good wear resistance, etc. Magnesium alloy is mainly used in aerospace, electronics and automobile fields. In order to improve the corrosion resistance of magnesium alloy devices, it is necessary to perform conversion film treatment on the surface of magnesium alloy to form a protective layer on the surface of magnesium alloy to improve the corrosion resistance of magnesium alloy.
[0003] However, although the phosphorus-free and chromium-free conversion coating treatment agents for magnesium alloys disclosed in the prior art anthologies, publications and patents improve the corrosion resistance of the magnesium alloy surface, the corrosion resistance time of the magnesium alloy is relatively short, that is, the time of neutral salt spray resistance is less than 24 hours, which is far from meeting the higher corrosion resistance requirements, thereby limiting the application field of magnesium alloys. In addition, the traditional phosphorus-free and chromium-free treatment agents for magnesium alloys contain pentavalent vanadates, which have high toxicity, are not only easy to pollute the environment, but also are not conducive to human health. Therefore, it is of great significance to develop a treatment agent with stable performance, environmental protection, and can significantly improve the corrosion resistance of the magnesium alloy surface. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a magnesium alloy titanium aluminum tungsten film treatment agent, a preparation method and a magnesium alloy surface treatment method which have stable performance, are environmentally friendly, and can significantly improve the corrosion resistance of the magnesium alloy surface without affecting the surface resistance and coating adhesion of the magnesium alloy titanium aluminum tungsten film.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A magnesium alloy titanium aluminum tungsten film treating agent, comprising the following components in the following concentrations:
[0007]
[0008] In some other embodiments, the following concentrations of each component are included:
[0009]
[0010] In some other embodiments, the following concentrations of each component are included:
[0011]
[0012] The balance is water. In some other embodiments, the molecular weight of the polyethylene glycol is 200-600.
[0013] In some other embodiments, the molecular weight of the polyethylene glycol is 400.
[0014] A method for preparing a magnesium alloy titanium aluminum tungsten coating treatment agent, wherein the magnesium alloy titanium aluminum tungsten coating treatment agent described in any of the above embodiments is obtained by using the preparation method, and the preparation method comprises the following steps:
[0015] Add 98% sulfuric acid into water and stir to obtain a mixed solution;
[0016] 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol are added to the mixed solution and stirred to obtain the magnesium alloy titanium aluminum tungsten coating treatment agent.
[0017] A magnesium alloy surface treatment method comprises using the magnesium alloy titanium aluminum tungsten coating treatment agent described in any of the above embodiments to perform surface treatment on the magnesium alloy, wherein the magnesium alloy titanium aluminum tungsten coating treatment agent is prepared using the preparation method described in any of the above embodiments.
[0018] In some other embodiments, the steps include:
[0019] Obtaining magnesium alloys;
[0020] Degreasing and deoiling the surface of the magnesium alloy;
[0021] Performing pickling and activation on the magnesium alloy after degreasing and deoiling treatment;
[0022] Performing surface conditioning and deashing treatment on the magnesium alloy after pickling and activation;
[0023] The magnesium alloy that has been subjected to surface conditioning and deashing treatment is placed in the magnesium alloy titanium aluminum tungsten coating treatment agent for immersion treatment;
[0024] performing a closed water washing treatment on the magnesium alloy that has undergone the immersion treatment;
[0025] The magnesium alloy that has undergone the closed water washing treatment is dried.
[0026] In some other embodiments, the soaking condition is room temperature and the time is 20 seconds to 35 seconds.
[0027] In some other embodiments, the thickness of the titanium-aluminum-tungsten film obtained by the magnesium alloy surface treatment method is 4 microns to 6 microns.
[0028] Compared with the prior art, the present invention has at least the following advantages:
[0029] 1. The above-mentioned magnesium alloy titanium aluminum tungsten film treating agent, since the formula of the magnesium alloy titanium aluminum tungsten film treating agent adopts 98% sulfuric acid 1 g / L to 4 g / L; 50% fluorotitanic acid 1 g / L to 3 g / L; aluminum nitrate 1 g / L to 5 g / L; ammonium metatungstate 0.5 g / L to 2 g / L; polyethylene glycol 0.2 g / L to 1 g / L; the balance is water; it can form a titanium aluminum tungsten film with stable performance on the surface of the magnesium alloy, and will not affect the surface resistance and coating adhesion of the magnesium alloy titanium aluminum tungsten film, thereby effectively improving the corrosion resistance of the magnesium alloy, and then improving the service life of the magnesium alloy, that is, the magnesium alloy still maintains good salt spray performance after continuous spraying of 5% sodium chloride neutral salt spray for more than 48 hours, and no black corrosion spots appear, which can meet higher corrosion resistance requirements, can improve the application field of the magnesium alloy, and improve the economic benefits of the magnesium alloy.
[0030] 2. The above-mentioned magnesium alloy titanium-aluminum-tungsten coating treatment agent does not contain pentavalent vanadate, thus avoiding the problem of traditional magnesium alloy phosphorus-free and chromium-free treatment agents often using pentavalent vanadium to pollute the environment and harm human health. It will not pollute the environment and has little harm to the human body, so that the magnesium alloy obtained after the magnesium alloy titanium-aluminum-tungsten coating treatment agent is not only environmentally friendly, but also has good corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 A flow chart of a method for preparing a magnesium alloy titanium aluminum tungsten coating treatment agent according to one embodiment of the present invention;
[0033] Figure 2 A flow chart of a magnesium alloy surface treatment method according to an embodiment of the present invention;
[0034] Figure 3 This is a diagram showing the appearance of the magnesium alloy subjected to continuous salt spray for 24 hours in Example 5 of the present invention;
[0035] Figure 4 This is a diagram showing the appearance of the magnesium alloy subjected to continuous salt spray for 48 hours according to Example 6 of the present invention;
[0036] Figure 5 This is a diagram showing the appearance of the magnesium alloy of Example 7 of the present invention subjected to continuous salt spray for 72 hours. DETAILED DESCRIPTION
[0037] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0038] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to suppress the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0040] For example, a magnesium alloy titanium aluminum tungsten coating treatment agent includes the following components in the following concentrations:
[0041] 98% sulfuric acid 1 g / L to 4 g / L;
[0042] 50% fluorotitanic acid 1 g / L to 3 g / L;
[0043] Aluminum nitrate 1 g / L to 5 g / L;
[0044] Ammonium metatungstate 0.5 g / L ~ 2 g / L;
[0045] Polyethylene glycol 0.2 g / L to 1 g / L;
[0046] The balance is water.
[0047] The above-mentioned magnesium alloy titanium aluminum tungsten film treating agent, as the formula of the magnesium alloy titanium aluminum tungsten film treating agent adopts 98% sulfuric acid 1 g / L to 4 g / L; 50% fluorotitanic acid 1 g / L to 3 g / L; aluminum nitrate 1 g / L to 5 g / L; ammonium metatungstate 0.5 g / L to 2 g / L; polyethylene glycol 0.2 g / L to 1 g / L; the balance is water; can form a layer of titanium aluminum tungsten film with stable performance on the surface of the magnesium alloy, and will not affect the surface resistance and coating adhesion of the magnesium alloy titanium aluminum tungsten film, thereby effectively improving the corrosion resistance of the magnesium alloy, and then improving the service life of the magnesium alloy, that is, the magnesium alloy still maintains good salt spray performance after continuous spraying of 5% sodium chloride neutral salt spray for more than 48 hours, and no black corrosion spots appear. For details, please refer to Figure 3 to Figure 5 ,from Figure 5 It can be seen that the appearance of the continuous fogging for 48 hours still has no black corrosion spots, indicating that the use of the magnesium alloy titanium aluminum tungsten film treatment agent of the present application can meet higher corrosion resistance requirements, can improve the application field of magnesium alloys, and improve the economic benefits of magnesium alloys. In addition, the above-mentioned magnesium alloy titanium aluminum tungsten film treatment agent does not contain pentavalent vanadates, thereby avoiding the problem of traditional magnesium alloy phosphorus-free and chromium-free treatment agents commonly using pentavalent vanadium to pollute the environment and harm human health. It will not pollute the environment and has little harm to the human body, so that the magnesium alloy obtained after the magnesium alloy titanium aluminum tungsten film treatment agent is not only environmentally friendly, but also has good corrosion resistance.
[0048] It should be noted that the applicant has discovered that if the concentration of 50% fluorotitanic acid is lower than 1 g / L, the concentration of aluminum nitrate is lower than 1 g / L, and the concentration of ammonium metatungstate is lower than 0.5 g / L, the integrity of the titanium-aluminum-tungsten film formed on the surface of the magnesium alloy is poor, resulting in poor corrosion resistance and salt spray resistance of the magnesium alloy. If the concentration of 50% fluorotitanic acid is higher than 3 g / L, the concentration of aluminum nitrate is higher than 5 g / L, and the concentration of ammonium metatungstate is higher than 2 g / L, the density and uniformity of the titanium-aluminum-tungsten film formed on the surface of the magnesium alloy are poor, resulting in poor corrosion resistance and salt spray resistance of the magnesium alloy. Therefore, the present application can form a complete, uniform, dense, stable, environmentally friendly, corrosion-resistant and salt-spray-resistant titanium-aluminum-tungsten film on the surface of the magnesium alloy by combining 50% fluorotitanic acid at 1 g / L to 3 g / L; aluminum nitrate at 1 g / L to 5 g / L; ammonium metatungstate at 0.5 g / L to 2 g / L with 98% sulfuric acid at 1 g / L to 4 g / L and polyethylene glycol at 0.2 g / L to 1 g / L.
[0049] It is worth mentioning that, since the raw materials of the entire system of the above-mentioned magnesium alloy titanium-aluminum-tungsten film treatment agent are all inorganic compounds, the bonding force between the titanium-aluminum-tungsten film and the magnesium alloy can be greatly improved, that is, fluorotitanic acid, aluminum nitrate and ammonium metatungstate can form a titanium-aluminum-tungsten film with high density, good firmness and stable performance on the surface of the magnesium alloy, while not affecting the surface resistance of the magnesium alloy conversion film and the adhesion of the coating. It is not only environmentally friendly, but also has good corrosion resistance and salt spray resistance, so that the magnesium alloy can maintain good salt spray performance after continuous salt spray for more than 48 hours, and no black corrosion spots appear. It should also be noted that after the magnesium alloy is treated with the magnesium alloy titanium-aluminum-tungsten film treatment agent of the present application, a light grayish white and uniform titanium-aluminum-tungsten film can be obtained, which not only improves the surface gloss of the magnesium alloy, but also improves the corrosion resistance and salt spray resistance of the magnesium alloy.
[0050] In some other embodiments, the concentration ratio of 50% fluorotitanic acid, aluminum nitrate and ammonium metatungstate is (1.5-2): (1.5-2): (1-2). In this way, the synergistic effect of the components of 50% fluorotitanic acid, aluminum nitrate and ammonium metatungstate is better, and a titanium-aluminum-tungsten film with better uniformity, density, corrosion resistance and salt spray resistance can be formed.
[0051] In some other embodiments, the molecular weight of the polyethylene glycol is 200-600. Since polyethylene glycol can play a good dispersing and wetting role, the addition of polyethylene glycol with a molecular weight of 200-600 not only plays a good dispersing and wetting role, but also facilitates 50% fluorotitanic acid, aluminum nitrate and ammonium metatungstate to form a dense, uniform and firm titanium-aluminum-tungsten film on the surface of the magnesium alloy. Further, in some other embodiments, the molecular weight of the polyethylene glycol is 400 to obtain a titanium-aluminum-tungsten film with better density, uniformity and firmness, and under electron microscope observation, the titanium-aluminum-tungsten film formed on the surface of the magnesium alloy has fewer holes and good overall density, thereby further improving the salt spray resistance and corrosion resistance of the magnesium alloy. Further, the water is deionized water.
[0052] Preferably, in one embodiment, the magnesium alloy titanium aluminum tungsten film treating agent includes the following components in concentrations: 98% sulfuric acid 2 g / L to 3 g / L; 50% fluorotitanic acid 2 g / L to 3 g / L; aluminum nitrate 2 g / L to 3 g / L; ammonium metatungstate 1 g / L to 2 g / L; polyethylene glycol 0.5 g / L to 1 g / L.
[0053] It can be understood that, through research by the applicant, it is found that by compounding 2 g / L to 3 g / L of 98% sulfuric acid; 2 g / L to 3 g / L of 50% fluorotitanic acid; 2 g / L to 3 g / L of aluminum nitrate; 1 g / L to 2 g / L of ammonium metatungstate; and 0.5 g / L to 1 g / L of polyethylene glycol, a titanium-aluminum-tungsten film with excellent uniformity, density, corrosion resistance and salt spray resistance can be generated on the surface of the magnesium alloy, so that the titanium-aluminum-tungsten film has no black corrosion spots after being continuously salt sprayed for more than 48 hours, thereby further improving the corrosion resistance of the magnesium alloy.
[0054] In a preferred embodiment, the magnesium alloy titanium aluminum tungsten film treatment agent includes the following components in the following concentrations: 1.5 g / L 98% sulfuric acid; 1.5 g / L 50% fluorotitanic acid; 1.5 g / L aluminum nitrate; 1 g / L ammonium metatungstate; 0.5 g / L polyethylene glycol. The applicant has found that the above-mentioned formula components are compounded and used, so that the titanium aluminum tungsten film is continuously subjected to salt spray for more than 48 hours without black corrosion spots, which further improves the corrosion resistance of the magnesium alloy.
[0055] In a more preferred embodiment, the magnesium alloy titanium aluminum tungsten film treating agent includes the following components in concentrations: 2.8 g / L of 98% sulfuric acid; 2.8 g / L of 50% fluorotitanic acid; 3 g / L of aluminum nitrate; 1.5 g / L of ammonium metatungstate; and 1 g / L of polyethylene glycol.
[0056] It can be understood that, through research by the applicant, it was found that by compounding 2.8 g / L of 98% sulfuric acid, 2.8 g / L of 50% fluorotitanic acid, 3 g / L of aluminum nitrate, 1.5 g / L of ammonium metatungstate, and 1 g / L of polyethylene glycol, a titanium-aluminum-tungsten film with better uniformity, density, corrosion resistance, and salt spray resistance can be generated on the surface of the magnesium alloy, so that the titanium-aluminum-tungsten film is subjected to continuous salt spray for more than 72 hours without showing black corrosion spots, thereby further improving the corrosion resistance of the magnesium alloy.
[0057] The present application also provides a method for preparing a magnesium alloy titanium aluminum tungsten coating treatment agent, and the preparation method is used to obtain the magnesium alloy titanium aluminum tungsten coating treatment agent described in any of the above embodiments, and the preparation method comprises the following steps: adding 98% sulfuric acid to water and stirring and mixing to obtain a mixed solution; adding 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol to the mixed solution and stirring and mixing to obtain the magnesium alloy titanium aluminum tungsten coating treatment agent. The above preparation method first adds 98% sulfuric acid to water and stirs and mixes, and then stirs and mixes 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol to obtain the magnesium alloy titanium aluminum tungsten coating treatment agent, and the operation is simple and fast.
[0058] See also Figure 2In order to better understand the technical solution and beneficial effects of the present application, the present application is further described in detail below in conjunction with specific examples. A method for preparing a magnesium alloy titanium aluminum tungsten coating treatment agent in one embodiment includes some or all of the following steps:
[0059] S110, adding 98% sulfuric acid into water, stirring and mixing, to obtain a mixed solution.
[0060] S120, adding 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol to the mixed solution and stirring and mixing, so as to quickly prepare the magnesium alloy titanium aluminum tungsten coating treatment agent, which is not only simple to operate but also fast.
[0061] In a preferred embodiment, 98% sulfuric acid is first added to water and stirred to mix, and then 50% fluorotitanic acid, polyethylene glycol, aluminum nitrate and ammonium metatungstate are added to the mixture in sequence, so that the added 50% fluorotitanic acid can be mixed with 98% sulfuric acid to form a relatively low concentration and stable acid system, and then the polyethylene glycol dispersant is added to disperse evenly, which helps to disperse the aluminum nitrate and ammonium metatungstate in the acid system to obtain a relatively stable magnesium alloy titanium-aluminum-tungsten film treatment agent, so that when the magnesium alloy is subsequently surface treated, a titanium-aluminum-tungsten film with good uniformity, density, corrosion resistance and salt spray resistance can be quickly formed on the surface of the magnesium alloy.
[0062] The present application also provides a magnesium alloy surface treatment method, comprising using the magnesium alloy titanium aluminum tungsten film treatment agent described in any of the above embodiments to perform surface treatment on the magnesium alloy, wherein the magnesium alloy titanium aluminum tungsten film treatment agent is obtained using the above preparation method.
[0063] It can be understood that the magnesium alloy titanium aluminum tungsten film treatment agent obtained by the preparation method of the present application is applied to the surface treatment of the magnesium alloy, and a layer of titanium aluminum tungsten film with stable performance can be formed on the surface of the magnesium alloy, and at the same time, the surface resistance and coating adhesion of the magnesium alloy titanium aluminum tungsten film will not be affected, thereby effectively improving the corrosion resistance of the magnesium alloy, and then improving the service life of the magnesium alloy, that is, the magnesium alloy still maintains good salt spray performance after continuous spraying of 5% sodium chloride neutral salt spray for more than 48 hours, and no black corrosion points appear, which can meet higher corrosion resistance requirements, and can improve the application field of magnesium alloys, so as to improve the economic benefits of magnesium alloys. In addition, the above-mentioned magnesium alloy titanium aluminum tungsten film treatment agent does not contain pentavalent vanadate, thereby avoiding the problem of traditional magnesium alloy phosphorus-free and chromium-free treatment agents commonly using pentavalent vanadium to pollute the environment and damage human health, and will not pollute the environment, and will cause little damage to the human body, so that the magnesium alloy obtained after the magnesium alloy titanium aluminum tungsten film treatment agent is not only environmentally friendly, but also has good corrosion resistance.
[0064] See also Figure 1In order to better understand the technical solution and beneficial effects of the present application, the present application is further described in detail below in conjunction with specific embodiments. A magnesium alloy surface treatment method according to one embodiment includes some or all of the following steps:
[0065] S100. Obtain magnesium alloy for backup.
[0066] S200, degreasing and deoiling the surface of the magnesium alloy.
[0067] It can be understood that the surface of the magnesium alloy is degreased and deoiled to remove oil stains and impurities on the surface of the magnesium alloy. In one embodiment, the step of degreasing and deoiling the surface of the magnesium alloy includes the following specific steps: placing the magnesium alloy in a degreasing and deoiling agent for immersion treatment. Specifically, the degreasing and deoiling agent includes the following components in concentrations: 15 g / L potassium hydroxide, 2 g / L EDTA disodium (Ethylenediaminetetraacetic acid disodium salt, disodium ethylenediaminetetraacetic acid), 20 g / L sodium pyrophosphate, 1.25 g / L TX-10 emulsifier, and 1 g / L sodium benzenesulfonate. In this way, the degreasing and deoiling agent obtained by compounding the components of the above concentrations can effectively remove oil stains and impurities on the surface of the magnesium alloy, so that the titanium aluminum tungsten film can be better attached to the surface of the magnesium alloy, thereby improving the bonding force between the titanium aluminum tungsten film and the surface of the magnesium alloy. Furthermore, the temperature when the magnesium alloy is placed in the degreasing and deoiling agent for degreasing and deoiling is 60°C, and the immersion treatment is 6 minutes to effectively and comprehensively remove the oil and impurities on the surface of the magnesium alloy. In one embodiment, the magnesium alloy immersed in the degreasing and deoiling agent is taken out and washed with water to remove the excess degreasing and deoiling agent on the surface of the magnesium alloy, which effectively avoids the degreasing and deoiling agent on the surface of the magnesium alloy from affecting the adhesion of the titanium aluminum tungsten film on the surface of the magnesium alloy to reduce the bonding force between the titanium aluminum tungsten film and the surface of the magnesium alloy, thereby ensuring that the titanium aluminum tungsten film has good adhesion to the surface of the magnesium alloy.
[0068] S300, performing pickling activation on the magnesium alloy after degreasing and deoiling.
[0069] It can be understood that the magnesium alloy after degreasing and deoiling is pickled and activated to remove impurities such as oxides on the surface of the magnesium alloy, while also improving the surface roughness of the magnesium alloy, thereby increasing the surface area of the magnesium alloy, so that when the magnesium alloy is subsequently surface treated with a magnesium alloy titanium-aluminum-tungsten film treatment agent, the titanium-aluminum-tungsten film can better adhere to the surface of the magnesium alloy, thereby improving the bonding strength between the magnesium alloy and the titanium-aluminum-tungsten film, thereby improving the corrosion resistance and salt spray resistance of the magnesium alloy.
[0070] Furthermore, the pickling agent is an M330 pickling agent, so that the M330 pickling agent can perform pickling activation on the magnesium alloy well, so as to effectively remove impurities such as oxides on the surface of the magnesium alloy, and at the same time improve the surface roughness of the magnesium alloy. Further, the M330 pickling agent is a product of Dongming Chemical in Boluo County. Further, the temperature of the pickling activation is 50 to 60°C; the treatment is 60 to 120 seconds. Further, in one of the embodiments, the magnesium alloy immersed in the pickling agent is taken out and washed with water to remove excess pickling agent on the surface of the magnesium alloy, so as to ensure that the titanium-aluminum-tungsten film can be directly attached and fixed on the surface of the magnesium alloy to form a titanium-aluminum-tungsten film with higher firmness.
[0071] S400, performing a surface conditioning and deashing treatment on the magnesium alloy after pickling and activation, so as to effectively remove impurities on the surface of the magnesium alloy and make the surface of the magnesium alloy uniform and shiny.
[0072] In some other embodiments, the step of performing surface conditioning and deashing treatment on the magnesium alloy after pickling and activation includes the following specific steps: the magnesium alloy after surface conditioning and deashing treatment is placed in a surface conditioning agent for surface conditioning and deashing treatment. Further, the surface conditioning and deashing treatment condition is a temperature of 25 to 60°C and a treatment time of 1 to 3 seconds, so that impurities in the magnesium alloy can be quickly removed and the surface of the magnesium alloy is uniform and shiny. Preferably, the surface conditioning agent is M440, which is a product of Dongming Chemical of Boluo County.
[0073] S500, the magnesium alloy that has undergone surface conditioning and deashing treatment is placed in the magnesium alloy titanium aluminum tungsten coating treatment agent for immersion treatment.
[0074] It can be understood that the magnesium alloy that has been treated with surface conditioning and deashing is placed in the magnesium alloy titanium aluminum tungsten film treatment agent for immersion treatment, which can form a layer of titanium aluminum tungsten film with stable performance on the surface of the magnesium alloy, and will not affect the surface resistance and coating adhesion of the magnesium alloy titanium aluminum tungsten film, thereby effectively improving the corrosion resistance of the magnesium alloy, and then improving the service life of the magnesium alloy, that is, the magnesium alloy still maintains good salt spray performance after continuous spraying of 5% sodium chloride neutral salt spray for more than 48 hours, and no black corrosion points appear, which can meet higher corrosion resistance requirements, and can improve the application field of magnesium alloys, so as to improve the economic benefits of magnesium alloys. In addition, the above-mentioned magnesium alloy titanium aluminum tungsten film treatment agent does not contain pentavalent vanadate, thereby avoiding the problem of traditional magnesium alloy phosphorus-free and chromium-free treatment agents commonly using pentavalent vanadium to pollute the environment and damage human health, and will not pollute the environment, and will cause little damage to the human body, so that the magnesium alloy obtained after the magnesium alloy titanium aluminum tungsten film treatment agent is not only environmentally friendly, but also has good corrosion resistance. Furthermore, the immersion condition is room temperature and the time is 20 seconds to 35 seconds, so as to quickly form a titanium aluminum tungsten film on the surface of the magnesium alloy.
[0075] S600, the magnesium alloy that has been immersed is subjected to a closed water washing treatment to better seal the holes of the titanium-aluminum-tungsten film, effectively preventing moisture or oxygen in the air from entering the holes of the titanium-aluminum-tungsten film to improve the stability of the titanium-aluminum-tungsten film, thereby improving the corrosion resistance and salt spray resistance of the magnesium alloy. Specifically, the magnesium alloy is sealed with an M600 sealant at a temperature of 50°C to 55°C for 2 to 3 minutes, and then washed with water to remove excess M600 sealant on the surface of the magnesium alloy. Furthermore, the M600 sealant is a chromium-free M600 sealant produced by Dongming Chemical in Boluo County.
[0076] S700, drying the magnesium alloy after the closed water washing treatment, drying the magnesium alloy after the closed water washing treatment to remove moisture on the surface of the magnesium alloy. Specifically, the magnesium alloy after the closed water washing treatment is placed in an oven at a temperature of 130° C. to 140° C. and continuously baked for 10 minutes to 25 minutes, so that the moisture of the magnesium alloy can be removed more quickly and effectively.
[0077] In some other embodiments, the titanium-aluminum-tungsten film obtained by the magnesium alloy surface treatment method has a thickness of 4 to 6 microns and a light grayish white color, which not only improves the appearance color of the magnesium alloy, but also improves the corrosion resistance and salt spray resistance of the magnesium alloy. At the same time, it will not affect the surface resistance and coating adhesion of the magnesium alloy titanium-aluminum-tungsten film, and is environmentally friendly, greatly improving the application field of magnesium alloys.
[0078] It should be noted that in order to form a chromium-free, vanadium-free, and phosphorus-free environmentally friendly titanium-aluminum-tungsten film on the surface of the magnesium alloy, the present application does not use chemical materials and production equipment containing chromium, vanadium, and phosphorus in the process of the magnesium alloy surface treatment method and the preparation method of the magnesium alloy titanium-aluminum-tungsten film treatment agent, thereby ensuring that the magnesium alloy can obtain a chromium-free, vanadium-free, and phosphorus-free environmentally friendly titanium-aluminum-tungsten film with good density, corrosion resistance, and salt spray resistance after surface treatment, thereby improving the corrosion resistance and salt spray resistance of the magnesium alloy. That is, the M600 sealant, M330 pickling agent, and M440 surface conditioning agent all contain chromium-free, vanadium-free, and phosphorus-free.
[0079] Some specific examples are given below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.
[0080] Table 1 is a table showing the concentration of each component of the magnesium alloy titanium aluminum tungsten coating treatment agent of Examples 1 to 7, in grams per liter.
[0081] Table 1
[0082]
[0083] The magnesium alloy titanium aluminum tungsten coating treatment agent component table of Examples 1 to 7 in Table 1 was prepared according to the following steps:
[0084] Add 98% sulfuric acid into water and stir to obtain a mixed solution;
[0085] 50% fluorotitanic acid, polyethylene glycol, aluminum nitrate and ammonium metatungstate were sequentially added to the mixed solution and stirred and mixed to obtain the magnesium alloy titanium aluminum tungsten coating treatment agents of different components of Examples 1 to 7 respectively.
[0086] The magnesium alloy titanium aluminum tungsten coating treatment agents prepared in Examples 1 to 7 are respectively applied to the magnesium alloy surface treatment method, which includes the following steps:
[0087] Obtain magnesium alloy; soak the magnesium alloy in a degreasing and deoiling agent at a temperature of 60°C for 6 minutes, wherein the degreasing and deoiling agent includes the following components in concentrations: 15 g / L potassium hydroxide, 2 g / L disodium EDTA, 20 g / L sodium pyrophosphate, 1.25 g / L TX-10 emulsifier, and 1 g / L sodium benzenesulfonate; after washing with water, soak the magnesium alloy in an M330 pickling agent at a temperature of 60°C for 90 seconds; after washing with water, soak the magnesium alloy in an M440 surface conditioning agent at a temperature of 45°C for 2 seconds; after washing with water, soak the magnesium alloy in a normal temperature magnesium alloy titanium aluminum tungsten coating treatment agent for 25 seconds; after washing with water, soak the magnesium alloy in an M600 sealing agent at a temperature of 55°C for 3 minutes; after washing with water, soak the magnesium alloy in an oven at 135°C for 15 minutes.
[0088] Comparative Example 1
[0089] Different from Example 7, the magnesium alloy titanium aluminum tungsten coating treatment agent includes the following components in concentration: 2.8 g / L 98% sulfuric acid, 3 g / L aluminum nitrate, 1.5 g / L ammonium metatungstate, 1 g / L polyethylene glycol and the balance is water.
[0090] Comparative Example 2
[0091] Different from Example 7, the magnesium alloy titanium aluminum tungsten coating treatment agent includes the following components in concentration: 2.8 g / L 98% sulfuric acid, 2.8 g / L 50% fluorotitanic acid, 1.5 g / L ammonium metatungstate, 1 g / L polyethylene glycol and the balance is water.
[0092] Comparative Example 3
[0093] Different from Example 7, the magnesium alloy titanium aluminum tungsten coating treatment agent includes the following components in concentration: 2.8 g / L 98% sulfuric acid, 2.8 g / L 50% fluorotitanic acid, 3 g / L aluminum nitrate, 1 g / L polyethylene glycol and the balance is water.
[0094] Comparative Example 4
[0095] Different from Example 7, the magnesium alloy titanium aluminum tungsten film treatment agent includes the following components in concentration: 0.9 g / L of 98% sulfuric acid, 3.1 g / L of 50% fluorotitanic acid, 5.1 g / L of aluminum nitrate, 2.1 g / L of ammonium metatungstate, 0.1 g / L of polyethylene glycol and the balance is water.
[0096] Comparative Example 5
[0097] Different from Example 7, the magnesium alloy titanium aluminum tungsten film treatment agent includes the following components in concentration: 4.1 g / L 98% sulfuric acid, 0.9 g / L 50% fluorotitanic acid, 0.9 g / L aluminum nitrate, 0.4 g / L ammonium metatungstate, 1.1 g / L polyethylene glycol and the balance is water.
[0098] After the magnesium alloy samples treated in Examples 1 to 7 and Comparative Examples 1 to 5 were placed at room temperature for 24 hours, a salt spray test was performed according to ASTM B-117. The samples were observed after continuous spraying. The experimental results are shown in Table 2:
[0099] Table 2
[0100]
[0101] From Table 2, it can be seen that the salt spray resistance of the magnesium alloy samples treated in Examples 1 to 7 is better than that of Comparative Examples 1 to 5, that is, the salt spray resistance time can reach more than 24 hours. The light gray-white titanium-aluminum-tungsten film with good adhesion, density and uniformity formed on the surface of the magnesium alloy by Examples 1 to 7 not only improves the appearance and color of the magnesium alloy, but also improves the corrosion resistance and salt spray resistance of the magnesium alloy, and is environmentally friendly. Further, the salt spray resistance of the magnesium alloy samples treated in Examples 3, 4, 6, and 7 can reach more than 48 hours, especially the best salt spray resistance of Example 7, which can reach more than 72 hours. For details, please refer to Figure 5 The figure shows the appearance of the magnesium alloy sample subjected to continuous salt spray for 72 hours.
[0102] The resistance test of the magnesium alloy samples after the treatment of Examples 1 to 7 and Comparative Examples 1 to 5 showed that the resistance test of the magnesium alloy workpieces of Examples 1 to 7 after the salt spray test was relatively stable, all less than 2Ω, while the resistance test of the magnesium alloy workpieces of the magnesium alloy samples of Comparative Examples 1 to 5 after the salt spray test showed an upward trend, all reaching more than 5Ω, with large fluctuations, that is, the stability of the aluminum tungsten film is poor. Among them, the resistance test conditions: the resistance test of the magnesium alloy workpiece after the salt spray test was performed using a resistance tester.
[0103] The adhesion test of the magnesium alloy samples treated in Examples 1 to 7 and Comparative Examples 1 to 5 showed that the 100-grid adhesion of the magnesium alloy samples in Examples 1 to 7 and Comparative Examples 4 to 5 was qualified, while the 100-grid adhesion of the magnesium alloy samples in Comparative Examples 1 to 3 was unqualified, that is, the adhesion was poor. The conditions for the adhesion test were: spraying paint on the treated magnesium alloy workpiece and testing the 100-grid adhesion.
[0104] Compared with the prior art, the present invention has at least the following advantages:
[0105] 1. The above-mentioned magnesium alloy titanium aluminum tungsten film treating agent, since the formula of the magnesium alloy titanium aluminum tungsten film treating agent adopts 98% sulfuric acid 1 g / L to 4 g / L; 50% fluorotitanic acid 1 g / L to 3 g / L; aluminum nitrate 1 g / L to 5 g / L; ammonium metatungstate 0.5 g / L to 2 g / L; polyethylene glycol 0.2 g / L to 1 g / L; the balance is water; it can form a titanium aluminum tungsten film with stable performance on the surface of the magnesium alloy, and will not affect the surface resistance and coating adhesion of the magnesium alloy titanium aluminum tungsten film, thereby effectively improving the corrosion resistance of the magnesium alloy, and then improving the service life of the magnesium alloy, that is, the magnesium alloy still maintains good salt spray performance after continuous spraying of 5% sodium chloride neutral salt spray for more than 48 hours, and no black corrosion spots appear, which can meet higher corrosion resistance requirements, can improve the application field of the magnesium alloy, and improve the economic benefits of the magnesium alloy.
[0106] 2. The above-mentioned magnesium alloy titanium-aluminum-tungsten coating treatment agent does not contain pentavalent vanadate, thus avoiding the problem of traditional magnesium alloy phosphorus-free and chromium-free treatment agents often using pentavalent vanadium to pollute the environment and harm human health. It will not pollute the environment and has little harm to the human body, so that the magnesium alloy obtained after the magnesium alloy titanium-aluminum-tungsten coating treatment agent is not only environmentally friendly, but also has good corrosion resistance.
[0107] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as a restriction on the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A magnesium alloy titanium aluminum tungsten film treatment agent, characterized in that: The following concentrations of components are included:
2. The magnesium alloy titanium aluminum tungsten coating treatment agent according to claim 1, characterized in that: The following concentrations of components are included:
3. The magnesium alloy titanium aluminum tungsten coating treatment agent according to claim 1, characterized in that: The following concentrations of components are included:
4. The magnesium alloy titanium aluminum tungsten coating treatment agent according to claim 1, characterized in that: The molecular weight of the polyethylene glycol is 200-600.
5. The magnesium alloy titanium aluminum tungsten coating treatment agent according to claim 4, characterized in that: The molecular weight of the polyethylene glycol is 400.
6. A method for preparing a magnesium alloy titanium aluminum tungsten coating treatment agent, characterized in that: The magnesium alloy titanium aluminum tungsten coating treatment agent according to any one of claims 1 to 5 is obtained by adopting the preparation method, and the preparation method comprises the following steps: Add 98% sulfuric acid into water and stir to obtain a mixed solution; 50% fluorotitanic acid, aluminum nitrate, ammonium metatungstate and polyethylene glycol are added to the mixed solution and stirred to obtain the magnesium alloy titanium aluminum tungsten coating treatment agent.
7. A method for surface treatment of magnesium alloy, characterized in that: The method comprises treating a magnesium alloy with the magnesium alloy titanium aluminum tungsten coating treatment agent described in any one of claims 1 to 5, wherein the magnesium alloy titanium aluminum tungsten coating treatment agent is prepared by the preparation method described in claim 6.
8. The magnesium alloy surface treatment method according to claim 7, characterized in that: The steps include: Obtaining magnesium alloys; Degreasing and deoiling the surface of the magnesium alloy; Performing pickling and activation on the magnesium alloy after degreasing and deoiling treatment; Performing surface conditioning and deashing treatment on the magnesium alloy after pickling and activation; The magnesium alloy that has been subjected to surface conditioning and deashing treatment is placed in the magnesium alloy titanium aluminum tungsten coating treatment agent for immersion treatment; performing a closed water washing treatment on the magnesium alloy that has undergone the immersion treatment; The magnesium alloy that has undergone the closed water washing treatment is dried.
9. The magnesium alloy surface treatment method according to claim 8, characterized in that: The soaking condition is room temperature and the soaking time is 20 seconds to 35 seconds.
10. The magnesium alloy surface treatment method according to any one of claims 7 to 9, characterized in that: The thickness of the titanium-aluminum-tungsten film obtained by the magnesium alloy surface treatment method is 4 microns to 6 microns.
Citation Information
Patent Citations
Aluminum treatment composition
CN102144042A
AZ31B magnesium alloy golden conversion film treatment agent and AZ31B magnesium alloy surface treatment method
CN109536941A
Conversion agent and treatment method for black conversion films of AZ91D die-casting magnesium alloys
CN111893469A
Black film formation treatment agent for metallic surface and treatment method therefor
JP2003213446A
Aluminum Treatment Composition
US20090242081A1