Indole sulfonated monomer, indole sulfonated polymer and proton exchange membrane and preparation method thereof

The proton exchange membrane is prepared by the acylation polymerization method of indole sulfonated monomers and phosphorus pentoxide, which solves the problems of low resistance to free radical oxidation and low conductivity in the existing technology, and achieves high performance and low cost. Proton exchange membrane preparation, suitable for large-scale applications.

CN116253673BActive Publication Date: 2024-10-18SHANDONG TIANWEI MEMBRANE TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310045708.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-30
Publication Date
2024-10-18
Estimated Expiration
2043-01-30

AI Technical Summary

Technical Problem

Existing proton exchange membranes have low radical oxidation resistance and low conductivity, and the preparation method is high-cost and cumbersome, which limits the large-scale application of non-fluorinated aromatic proton exchange membranes.

Method used

Indole sulfonated polymers are prepared by using indole sulfonated monomers through sulfonation reactions and hydrolysis reactions to avoid free radical attacks caused by the presence of ether bonds. Phosphorus pentoxide and methylsulfonic acid are combined for acylation polymerization to form Proton exchange membrane with high mechanical strength and high electrical conductivity.

Benefits of technology

It achieves high oxidation resistance, mechanical strength and high conductivity of the proton exchange membrane, reduces the preparation cost, is suitable for large-scale production, and improves the performance and application prospects of non-fluorinated aromatic proton exchange membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116253673B_ABST
    Figure CN116253673B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of high-performance polymers, and specifically relates to an indole sulfonated monomer, an indole sulfonated polymer, a proton exchange membrane, and a preparation method thereof. The indole sulfonated monomer of the present invention is used as a raw material for preparing an indole sulfonated polymer and a proton exchange membrane. Due to the presence of an indole ring and the absence of sites such as ether bonds that are easily attacked by free radicals, the indole sulfonated polymer has strong resistance to free radical oxidation and swelling resistance. After experimental testing, the prepared proton exchange membrane has strong resistance to free radical oxidation, mechanical strength, and swelling resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance polymers, and specifically relates to an indole sulfonated monomer, an indole sulfonated polymer and a proton exchange membrane and a preparation method thereof. Background Art

[0002] As the core component of proton exchange membrane fuel cells, proton exchange membrane (PEM) is widely used in aerospace, energy conversion and storage, automotive industry, etc. Among them, perfluorosulfonic acid proton exchange membrane is widely used due to its advantages such as good chemical stability and thermal stability, voltage reduction, high conductivity, and high mechanical strength.

[0003] However, perfluorosulfonic acid proton exchange membrane also has certain defects. For example, its water content seriously affects the proton conductivity. The conductivity of the membrane will rapidly increase as the water content decreases. In addition, temperature will also have a great impact on the conductivity of the membrane. The conductivity of the membrane will decrease with increasing temperature. When the temperature is too high, the perfluorosulfonic acid proton exchange membrane will even hydrolyze. Not only that, the cost of perfluorosulfonic acid proton exchange membrane is too high, which is not conducive to industrial application. Therefore, finding a substitute for perfluorosulfonic acid proton exchange membrane has become an important research direction.

[0004] At present, PEM based on aromatic polymers is widely considered to be a very promising alternative to perfluorosulfonic acid proton exchange membranes. Existing research has made significant progress and many beneficial common conclusions in the relationship between the structural design of aromatic PEM and membrane performance. For example, compared with general main chain PEM, side chain PEM has higher conductivity and lower swelling degree; reducing ether oxygen structure can improve the oxidation stability of PEM; increasing nitrogen heteroaromatic ring can reduce the swelling degree of PEM, etc.

[0005] In recent years, polyphenylene with a full aromatic ring main chain, especially sulfonated polyphenylene prepared by DA reaction polymerization (Diels-Alder reaction) between alkynyl and sulfonated aromatic substituted diene ketone functional groups, has shown excellent comprehensive performance as a proton exchange membrane material and has been produced on a certain scale (for example, Pemion proton exchange membrane produced by Ionomr, Canada). However, the DA reaction polymerization method has the disadvantages of high price of alkynyl and diene ketone monomers, complicated synthesis steps, and high polymerization temperature. Other preparation methods such as metal-catalyzed coupling polymerization generally have the disadvantages of high price of metal catalysts and difficult post-processing. Therefore, it is still urgent to develop low-cost polymerization routes and methods that meet high performance requirements to further promote the large-scale application of non-fluorinated aromatic proton exchange membranes. For example, a Chinese invention patent with application publication number CN103044292A discloses a polyketone containing a sulfonated aromatic group and a preparation method thereof, specifically disclosing the use of a mixture of phosphorus pentoxide and methanesulfonic acid to catalyze an acylation polymerization reaction of a sulfonated aromatic compound containing an ether bond to prepare a side chain sulfonated polyketone. However, due to the presence of the ether bond, an ether oxygen structure exists in the structure of the obtained polymer, which reduces the free radical oxidation resistance of the obtained proton exchange membrane, and the conductivity of the obtained proton exchange membrane is relatively low. Summary of the invention

[0006] The object of the present invention is to provide an indole sulfonated monomer, which can solve the shortcomings of low free radical oxidation resistance and low conductivity of the proton exchange membrane prepared in the prior art when used for preparing the proton exchange membrane.

[0007] The second object of the present invention is to provide a method for preparing an indole sulfonated monomer, an indole sulfonated polymer prepared using the above-mentioned indole sulfonated monomer, a method for preparing an indole sulfonated polymer and a method for preparing a proton exchange membrane, so as to solve the shortcomings of the proton exchange membrane prepared in the prior art, such as low resistance to free radical oxidation and low conductivity.

[0008] In order to achieve the above purpose, an indole sulfonated monomer of the present invention has a structure as shown in Formula 1:

[0009]

[0010] R1 in Formula 1 is -(CH2) n -, n is 3 or 4, G1 is -SO3M; M in -SO3M and -OM in Formula 1 are both selected from any one atom of Li, Na, K or H.

[0011] The indole sulfonated monomer proposed in the present invention is used as a raw material for synthesizing a sulfonated polymer used for an aromatic proton exchange membrane. Since it does not contain sites such as ether bonds that are easily attacked by free radicals, it has a strong resistance to free radical oxidation. The presence of the indole ring can also reduce the swelling degree of the synthesized sulfonated polymer.

[0012] The invention discloses a method for preparing an indole sulfonated monomer, comprising the following steps: firstly mixing indole-6-carboxylate, alkali metal alkoxide and sultone for sulfonation reaction, then adding alkaline aqueous solution to the sulfonation reaction product for hydrolysis reaction, or adding alkaline aqueous solution to the sulfonation reaction product for hydrolysis reaction, then using acidic cation exchange resin to perform ion exchange on the hydrolysis reaction product; wherein the sultone is 1,3-propyl sultone or 1,4-butyl sultone.

[0013] The preparation method of the indole sulfonated monomer proposed by the present invention utilizes an alkali metal alkoxide to provide an alkaline environment, performs a sulfonation reaction on indole-6-carboxylate and sultone, realizes the sulfonation treatment on the indole ring, and then hydrolyzes the ester group under alkaline conditions to obtain the indole sulfonated monomer. The preparation method is simple and the preparation cost is low. The obtained indole sulfonated monomer is used as a raw material for the sulfonated polymer used for synthesizing an aromatic proton exchange membrane. Since it does not contain sites such as ether bonds that are easily attacked by free radicals, it has strong resistance to free radical oxidation. The presence of the indole ring can also reduce the swelling degree of the synthesized sulfonated polymer.

[0014] Preferably, the indole-6-carboxylic acid ester can be selected from any one of indole-6-carboxylic acid methyl ester, indole-6-carboxylic acid ethyl ester and indole-6-carboxylic acid propyl ester.

[0015] Preferably, the temperature of the sulfonation reaction is 30 to 100° C., and the reaction time is 2 to 24 hours.

[0016] Preferably, the temperature of the hydrolysis reaction is 60 to 80° C., and the reaction time is 8 to 12 hours.

[0017] The molar ratio of indole-6-carboxylate to alkali metal alkoxide is 1:1 to 1.5; the molar ratio of indole-6-carboxylate to sultone is 1:1 to 1.3. Preferably, the molar ratio of indole-6-carboxylate to tert-butoxide is 1:1 to 1.1; the molar ratio of indole-6-carboxylate to sultone is 1:1 to 1.05.

[0018] Preferably, the alkali metal alkoxide is tert-butoxide; the tert-butoxide is selected from lithium tert-butoxide, sodium tert-butoxide or potassium tert-butoxide; those skilled in the art should know that the alkaline aqueous solution is an aqueous solution of the hydroxide of the metal corresponding to the alkali metal alkoxide.

[0019] Preferably, the alkaline aqueous solution is an aqueous solution of lithium hydroxide, sodium hydroxide or potassium hydroxide, the mass concentration of the alkaline aqueous solution is 10-50%, and the molar ratio of indole-6-carboxylate to the alkali metal hydroxide in the alkaline aqueous solution is 1:1.1-2.25, preferably, the molar ratio is 1:1.3-1.5.

[0020] Furthermore, the alkali metal alkoxide is tert-butoxide, the tert-butoxide is potassium tert-butoxide, and the alkaline aqueous solution is an aqueous solution of potassium hydroxide.

[0021] Preferably, the solvent used in the sulfonation reaction is dimethyl sulfoxide, and the amount of dimethyl sulfoxide added is 5 to 60 mL of dimethyl sulfoxide per gram of indole-6-carboxylate. Further, the amount of dimethyl sulfoxide added is 10 to 30 mL of dimethyl sulfoxide per gram of indole-6-carboxylate.

[0022] Preferably, the preparation method of the indole sulfonated monomer further comprises the following steps: after the hydrolysis reaction, adding anhydrous ethanol to the product, filtering, then recrystallizing with 85-95% ethanol, and drying to obtain the indole sulfonated monomer. The amount of anhydrous ethanol added is 5 to 50 times the mass of the alkaline aqueous solution.

[0023] The indole sulfonated polymer of the present invention comprises a structural unit as shown in Formula 2:

[0024]

[0025] R2 in formula 2 is -(CH2) n -, n is 3 or 4, G2 is -SO3Q, and Q is a cation.

[0026] The indole sulfonated polymer proposed by the present invention has a simple structure and has strong resistance to free radical oxidation because it does not contain sites such as ether bonds that are easily attacked by free radicals. Generally, the higher the ion exchange capacity in the polymer, the higher the conductivity of the resulting proton exchange membrane, but the mechanical strength and swelling resistance will be greatly reduced. The main chain of the indole sulfonated polymer proposed by the present invention is completely composed of a rigid indole ring connected to a carbonyl group, so that the proton exchange membrane formed by the indole sulfonated polymer has high mechanical strength and excellent swelling resistance, and at the same time, the high ion exchange capacity gives the proton exchange membrane a higher conductivity.

[0027] Preferably, the cation Q corresponding to the sulfate anion on the indole sulfonated polymer is a proton. Further, the ion exchange method known in the art of ion exchange can be used to realize the conversion to other cations such as Li + 、Na + , K + NH4 + Plasma conversion.

[0028] Preferably, the indole sulfonated polymer proposed in the present invention further comprises a structural unit as shown in Formula 3:

[0029]

[0030] R3 in the structural unit shown in Formula 3 is selected from -H or a C1-C10 straight-chain alkyl group.

[0031] Preferably, the molecular weight of the above-mentioned indole sulfonated polymer is characterized by inherent logarithmic viscosity, and the inherent logarithmic viscosity of the indole sulfonated polymer is 1.0-6.0 dL / g; wherein, the inherent logarithmic viscosity is measured by the following steps: using 99% pure methanesulfonic acid as a solvent, the indole sulfonated polymer is prepared into a solution with a concentration of 0.3 g / 100 mL, and the inherent logarithmic viscosity is measured using an Ubbelohde viscometer at a temperature of 30°C.

[0032] The invention discloses a method for preparing an indole sulfonated polymer, comprising the following steps: subjecting reaction monomers to polymerization reaction under the catalytic action of phosphorus pentoxide and methanesulfonic acid; the reaction monomers include the above-mentioned indole sulfonated monomers.

[0033] The preparation method of the indole sulfonated polymer proposed by the present invention uses phosphorus pentoxide and methanesulfonic acid as catalysts to carry out a acylation reaction to generate the indole sulfonated polymer. The preparation method is simple, the preparation conditions are mild, and no metal catalyst needs to be introduced. In addition, the obtained polymer does not contain sites such as ether bonds that are easily attacked by free radicals, and has strong resistance to free radical oxidation. The main chain of the polymer is completely composed of an indole ring connected to a carbonyl group, which ensures high mechanical strength and swelling resistance of the polymer.

[0034] Preferably, the various indole sulfonated monomers included in the reaction monomers may be the same or different.

[0035] Preferably, the reactive monomer further comprises a comonomer as shown in Formula 4:

[0036]

[0037] R4 in the comonomer shown in Formula 4 is selected from -H or a C1-C10 straight-chain alkyl group. Preferably, the comonomers included in the reactive monomers may be the same or different.

[0038] Furthermore, the molar number of the comonomer is less than 5 times that of the indole sulfonated monomer. By adjusting the ratio of the indole sulfonated monomer to the comonomer, the ion exchange capacity of the indole sulfonated polymer can be precisely controlled.

[0039] Preferably, a mixture of phosphorus pentoxide and methanesulfonic acid can be obtained in advance, and then the reaction monomer and the mixture of phosphorus pentoxide and methanesulfonic acid are mixed to carry out polymerization reaction. Furthermore, the mixture of phosphorus pentoxide and methanesulfonic acid can be a commercial product or homemade, and the preparation method is as follows: phosphorus pentoxide and methanesulfonic acid are mixed in proportion.

[0040] Preferably, the weight ratio of phosphorus pentoxide to methanesulfonic acid is 7 to 10:100. The ratio of the mass of the reaction monomer to the total mass of phosphorus pentoxide and methanesulfonic acid is 5 to 30:100.

[0041] Preferably, the polymerization reaction is carried out under anhydrous conditions in order to avoid failure caused by reaction of phosphorus pentoxide with water during the reaction process.

[0042] Preferably, the polymerization reaction temperature is 30 to 100° C., and the reaction time is 2 to 24 hours.

[0043] The method for preparing a proton exchange membrane of the present invention comprises the following steps: coating a solution containing the above-mentioned indole sulfonated polymer on the surface of a substrate, and removing the solvent to obtain the proton exchange membrane.

[0044] The proton exchange membrane proposed in the present invention is prepared by using the above-mentioned indole sulfonated polymer, in which the cation corresponding to the sulfonate anion can be exchanged with other cations (such as H + 、Na + , K + The proton conductivity of the proton exchange membrane can reach 150mS / cm at 30°C and 288mS / cm at 80°C, which is a high conductivity. In addition, since the polymer main chain is completely composed of nitrogen-containing fused rings connected with carbonyl groups and does not contain sites such as ether bonds that are susceptible to free radical attack, the electrolyte membrane has high oxidation resistance, mechanical strength and swelling resistance, and has great application prospects in proton exchange membrane fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the indole sulfonated monomer prepared in Example 3 of the present invention;

[0046] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the indole sulfonated polymer prepared in Example 13 of the present invention;

[0047] Figure 3 is the hydrogen nuclear magnetic resonance spectrum of the indole sulfonated polymer of Example 14 of the present invention;

[0048] Figure 4is the hydrogen nuclear magnetic resonance spectrum of the comonomer 1-ethyl-6-indolecarboxylic acid of the present invention;

[0049] Figure 5 This is the hydrogen nuclear magnetic resonance spectrum of the product obtained in Experimental Example 1 of the present invention. DETAILED DESCRIPTION

[0050] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0051] When the comonomer used in the present invention is 1-ethyl-6-indolecarboxylic acid, 1-ethyl-6-indolecarboxylic acid can be prepared by the following steps: indole-6-carboxylic acid methyl ester (17.52g, 0.1mol), sodium tert-butoxide (10.57g, 0.11mol), ethyl bromide (10.9g, 0.1mol) and dimethyl sulfoxide (100mL) are added to a reaction bottle, reacted at a temperature of 30°C for 24 hours, then sodium hydroxide aqueous solution (15g, 40wt%) is added, hydrolysis reaction is carried out at a temperature of 80°C for 24 hours, then 0.5mol / L dilute hydrochloric acid is added until the pH of the reaction solution is about 4, and the reaction solution is allowed to stand. The resulting precipitate is filtered and recrystallized with 50% ethanol, and finally dried to obtain the comonomer 1-ethyl-6-indolecarboxylic acid.

[0052] The H NMR spectrum of the obtained comonomer 1-ethyl-6-indolecarboxylic acid is as follows: Figure 4 As shown, the results are as follows: 1 HNMR(400MHz, DMSO-d6)12.59(s,1H), δ8.10(s,1H),7.62(m,3H),6.52(d,1H),4.30(q,2H),1.37(t,3H).

[0053] The nuclear magnetic resonance hydrogen spectrum ( 1 H NMR was recorded on a Bruker AVANCE AV400 nuclear magnetic resonance spectrometer using deuterated water (D2O) or deuterated dimethyl sulfoxide (DMSO-d6, tetramethylsilane as internal standard) as solvent.

[0054] 1. The embodiments of the indole sulfonated monomers of the present invention are as follows:

[0055] Example 1

[0056] The structure of the indole sulfonated monomer of this embodiment is shown in Formula 5. The indole sulfonated monomer of this embodiment is prepared by the preparation method of the indole sulfonated monomer in Example 3.

[0057]

[0058] Example 2

[0059] The structure of the indole sulfonated monomer of this embodiment is shown in Formula 6. The indole sulfonated monomer of this embodiment is prepared by the preparation method of the indole sulfonated monomer in Example 4.

[0060]

[0061] 2. The embodiment of the preparation method of the indole sulfonated monomer of the present invention is as follows:

[0062] Example 3

[0063] The preparation method of the indole sulfonated monomer prepared in this embodiment is the preparation method of the indole sulfonated monomer in Example 1, which specifically comprises the following steps: adding indole-6-carboxylic acid methyl ester (17.52 g, 0.1 mol), potassium tert-butoxide (17.52 g, 0.1 mol), 1,3-propyl sultone (17.52 g, 0.1 mol) and dimethyl sulfoxide (175 mL) into a reaction bottle, reacting at a temperature of 60° C. for 18 hours, and then removing dimethyl sulfoxide by rotary evaporation.

[0064] A potassium hydroxide aqueous solution (26.88 g, 25 wt%) was added to the reaction product, and the reaction was hydrolyzed at 80° C. for 8 hours, and then anhydrous ethanol (134.40 g) was added for suction filtration. The resulting precipitate was recrystallized with 90% ethanol, and finally vacuum dried at 100° C. for 36 hours to obtain the indole sulfonated monomer in Example 1. The hydrogen nuclear magnetic resonance spectrum of the obtained indole sulfonated monomer is shown in FIG. Figure 1 As shown, the results are as follows: 1 H NMR (400MHz, D2O) δ7.99(s,1H),7.62(m,2H),7.37(d,1H),6.53(d,1H),4.29(t,2H),2.78(t,2H),2.22(m,2H).

[0065] Example 4

[0066] The preparation method of the indole sulfonated monomer prepared in this embodiment is the preparation method of the indole sulfonated monomer in Example 2, which specifically comprises the following steps: adding indole-6-carboxylic acid methyl ester (17.52 g, 0.1 mol), sodium tert-butoxide (10.57 g, 0.11 mol), 1,4-butyl sultone (14.3 g, 0.105 mol) and dimethyl sulfoxide (88 mL) into a reaction bottle, reacting at a temperature of 100° C. for 2 hours, and then removing dimethyl sulfoxide by rotary evaporation.

[0067] A sodium hydroxide aqueous solution (90 g, 10 wt%) was added to the reaction product, and the hydrolysis reaction was carried out at a temperature of 60° C. for 12 hours, and then anhydrous ethanol (4500 g) was added for suction filtration. The obtained precipitate was recrystallized with 90% ethanol, and finally vacuum dried at 100° C. for 36 hours to obtain the indole sulfonated monomer in Example 2. The test results of the nuclear magnetic resonance hydrogen spectrum of the obtained indole sulfonated monomer are as follows: 1 H NMR (400MHz, D2O) δ7.98(s,1H),7.63(m,2H),7.37(d,1H),6.53(d,1H),4.29(t,2H),2.76(t,2H),2.25(m,4H).

[0068] 3. Examples of the indole sulfonated polymers of the present invention are as follows:

[0069] The inherent logarithmic viscosity of the indole sulfonated polymer in Examples 5-10 was measured by the following steps: using 99% pure methanesulfonic acid as solvent, the indole sulfonated polymer was prepared into a solution with a concentration of 0.3 g / 100 mL, and the inherent logarithmic viscosity was measured using an Ubbelohde viscometer at a temperature of 30°C.

[0070] Example 5

[0071] The structural unit of the indole sulfonated polymer of this embodiment is shown in Formula 7. The measured inherent viscosity of the indole sulfonated polymer is 6.0 dL / g. The indole sulfonated polymer of this embodiment is prepared by the preparation method of the indole sulfonated polymer in Example 11.

[0072]

[0073] Example 6

[0074] The structural units of the indole sulfonated polymer of this embodiment are shown in Formula 7 and Formula 8. The measured inherent viscosity of the indole sulfonated polymer is 2.9 dL / g. The indole sulfonated polymer of this embodiment is prepared by the preparation method of the indole sulfonated polymer in Example 12.

[0075]

[0076] Example 7

[0077] The structural units of the indole sulfonated polymer of this embodiment are shown in Formula 7 and Formula 8. The measured inherent viscosity of the indole sulfonated polymer is 3.7 dL / g. The indole sulfonated polymer of this embodiment is prepared by the preparation method of the indole sulfonated polymer in Example 13.

[0078] Example 8

[0079] The structural units of the indole sulfonated polymer of this embodiment are shown in Formula 7 and Formula 8. The measured inherent viscosity of the indole sulfonated polymer is 4.3 dL / g. The indole sulfonated polymer of this embodiment is prepared by the preparation method of the indole sulfonated polymer in Example 14.

[0080] Example 9

[0081] The structural units of the indole sulfonated polymer of this embodiment are shown in Formula 7 and Formula 9. The measured inherent viscosity of the indole sulfonated polymer is 3.5 dL / g. The indole sulfonated polymer of this embodiment is prepared by the preparation method of the indole sulfonated polymer in Example 15.

[0082]

[0083] Example 10

[0084] The structural units of the indole sulfonated polymer of this embodiment are shown in Formula 10 and Formula 11, and the measured inherent viscosity of the indole sulfonated polymer is 1.0 dL / g. The indole sulfonated polymer of this embodiment is prepared by the preparation method of the indole sulfonated polymer in Example 16.

[0085]

[0086]

[0087] 4. The preparation method of the indole sulfonated polymer of the present invention is as follows:

[0088] Embodiment 11

[0089] The preparation method of the indole sulfonated polymer of this embodiment is the preparation method of the indole sulfonated polymer in Example 5, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 3000g of the indole sulfonated monomer in Example 1, 10000g of a mixture of phosphorus pentoxide and methanesulfonic acid (phosphorus pentoxide and methanesulfonic acid weight ratio is 10:100) are added into the glass reactor with nitrogen, mechanically stirred at a temperature of 100°C, reacted for 2 hours, and then the obtained viscous reaction liquid is slowly added into water, allowed to stand, the obtained precipitate is extracted with water through an extractor for 24 hours, and finally vacuum dried at a temperature of 100°C for 24 hours to obtain the indole sulfonated polymer. The polymerization reaction formula is as follows:

[0090]

[0091] Example 12

[0092] The preparation method of the indole sulfonated polymer of this embodiment is the preparation method of the indole sulfonated polymer in Example 6, which specifically includes the following steps: nitrogen is introduced into the glass reactor to replace the air, and then 359.5g (1mol) of the indole sulfonated monomer in Example 1, 806.0g (5mol) of 6-indolecarboxylic acid, 23310g of a mixture of phosphorus pentoxide and methanesulfonic acid (the weight ratio of phosphorus pentoxide to methanesulfonic acid is 7:100) are added to the glass reactor with nitrogen, mechanically stirred at a temperature of 30°C, reacted for 24 hours, and then the obtained viscous reaction liquid is slowly added to water, allowed to stand, and the obtained precipitate is extracted with water through an extractor for 24 hours, and finally vacuum dried at a temperature of 100°C for 24 hours to obtain the indole sulfonated polymer. The polymerization reaction formula is as follows:

[0093]

[0094] Embodiment 13

[0095] The preparation method of the indole sulfonated polymer of this embodiment is the preparation method of the indole sulfonated polymer in Example 7, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 359.5g (1mol) of the indole sulfonated monomer in Example 1, 161.2g (1mol) of 6-indolecarboxylic acid, and 5207g of a mixture of phosphorus pentoxide and methanesulfonic acid (the weight ratio of phosphorus pentoxide to methanesulfonic acid is 8.5:100) are added to the glass reactor passed with nitrogen, and the reaction is carried out by mechanical stirring at a temperature of 80°C for 12 hours, and then the obtained viscous reaction liquid is slowly added to water, and the mixture is allowed to stand, and the obtained precipitate is extracted with water through an extractor for 24 hours, and finally vacuum dried at a temperature of 100°C for 24 hours to obtain the indole sulfonated polymer.

[0096] The hydrogen nuclear magnetic resonance spectrum of the indole sulfonated polymer prepared in this example is as follows: Figure 2 As shown, it indicates that the molar ratio of the structural unit introduced by the indole sulfonated monomer to the structural unit introduced by the comonomer 6-indolecarboxylic acid is 1:1, which is consistent with the molar ratio of the initially added sulfonated monomer to the comonomer.

[0097] Embodiment 14

[0098] The preparation method of the indole sulfonated polymer of this embodiment is the preparation method of the indole sulfonated polymer in Example 8, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 719.0 g (2 mol) of the indole sulfonated monomer in Example 1, 161.2 g (1 mol) of 6-indolecarboxylic acid, and 8802 g of a mixture of phosphorus pentoxide and methanesulfonic acid (the weight ratio of phosphorus pentoxide to methanesulfonic acid is 8.5:100) are added to the glass reactor passed with nitrogen, mechanically stirred at a temperature of 80° C., reacted for 12 hours, and then the obtained viscous reaction liquid was slowly added to water, allowed to stand, and the obtained precipitate was extracted with water through an extractor for 24 hours, and finally vacuum dried at a temperature of 100° C. for 24 hours to obtain the indole sulfonated polymer.

[0099] The nuclear magnetic resonance hydrogen spectrum of the indole sulfonated polymer of this example is as follows Figure 3 As shown, the molar ratio of the structural unit introduced by the indole sulfonated monomer to the structural unit introduced by the comonomer 6-indolecarboxylic acid is 2:1, which is consistent with the molar ratio of the initially added sulfonated monomer to the comonomer.

[0100] Embodiment 15

[0101] The preparation method of the indole sulfonated polymer of this embodiment is the preparation method of the indole sulfonated polymer in Example 9, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 359.5g (1mol) of the indole sulfonated monomer in Example 1, 175.2g (1mol) of 1-methyl-6-indolecarboxylic acid, and 5347g of a mixture of phosphorus pentoxide and methanesulfonic acid (the weight ratio of phosphorus pentoxide to methanesulfonic acid is 8.0:100) are added into the glass reactor with nitrogen, mechanically stirred at a temperature of 80°C, reacted for 18 hours, and then the obtained viscous reaction liquid is slowly added into water, allowed to stand, and the obtained precipitate is extracted with water through an extractor for 24 hours, and finally vacuum dried at a temperature of 100°C for 24 hours to obtain the indole sulfonated polymer. The polymerization reaction formula is as follows:

[0102]

[0103] Example 16

[0104] The preparation method of the indole sulfonated polymer of this embodiment is the preparation method of the indole sulfonated polymer in Example 10, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 1438g (4mol) of the indole sulfonated monomer in Example 2, 301.4g (1mol) of 1-decyl-6-indolecarboxylic acid, and 34788g of a mixture of phosphorus pentoxide and methanesulfonic acid (the weight ratio of phosphorus pentoxide to methanesulfonic acid is 7.0:100) are added into the glass reactor with nitrogen, mechanically stirred at a temperature of 100°C, reacted for 8 hours, and then the obtained viscous reaction liquid is slowly added into water, allowed to stand, and the obtained precipitate is extracted with water through an extractor for 24 hours, and finally vacuum dried at a temperature of 100°C for 24 hours to obtain the indole sulfonated polymer. The polymerization reaction formula is shown below:

[0105]

[0106] The comonomer 1-decyl-6-indolecarboxylic acid used in this embodiment was prepared by the following steps: indole-6-carboxylic acid methyl ester (17.52 g, 0.1 mol), sodium tert-butoxide (10.57 g, 0.11 mol), 1-bromodecane (22.12 g, 0.1 mol) and dimethyl sulfoxide (150 mL) were added to a reaction flask, reacted at 80° C. for 24 hours, and then sodium hydroxide aqueous solution (15 g, 40 wt %) was added, and hydrolysis reaction was carried out at 80° C. for 24 hours, followed by adding 0.5 mol / L dilute hydrochloric acid until the pH of the reaction solution was about 4, and the reaction solution was allowed to stand. The resulting precipitate was filtered and recrystallized with acetone, and finally dried to obtain the comonomer 1-decyl-6-indolecarboxylic acid.

[0107] V. The preparation method of the proton exchange membrane of the present invention is as follows:

[0108] Embodiment 17

[0109] The preparation method of the proton exchange membrane of this embodiment includes the following steps: dissolving 1.0 g of the indole sulfonated polymer obtained in Example 7 in 15 mL of dimethyl sulfoxide, pouring the obtained solution onto a clean horizontal glass plate, placing it at 60°C for 24 hours to volatilize the dimethyl sulfoxide, then peeling the membrane from the glass plate, placing it in a vacuum drying oven at 80°C for 12 hours to remove the residual dimethyl sulfoxide solvent, and obtaining a layer of brown-red, transparent and flexible proton exchange membrane.

[0110] Embodiment 18

[0111] The preparation method of the proton exchange membrane of this embodiment includes the following steps: dissolving 1.0 g of the indole sulfonated polymer obtained in Example 10 in 20 mL of dimethylacetamide, then pouring the obtained solution onto a clean horizontal glass plate, placing it at 60°C for 24 hours to volatilize the dimethylacetamide, then peeling the membrane from the glass plate, placing it in a vacuum drying oven at 80°C for 12 hours to remove the residual solvent, and obtaining a layer of brown, transparent and flexible proton exchange membrane.

[0112] 6. Experimental Examples

[0113] Experimental Example 1

[0114] This experimental example is used to verify the feasibility of preparing indole sulfonated polymers by using indole sulfonated monomers, comonomers, and a mixture of phosphorus pentoxide and methanesulfonic acid through a acylation reaction in the present invention. 6-indolecarboxylic acid methyl ester, 4-methoxybenzoic acid, and a mixture of phosphorus pentoxide and methanesulfonic acid are used as raw materials for the reaction, specifically as follows: 0.832g (4.75mmol) of 6-indolecarboxylic acid methyl ester, 1.445g (9.50mmol) of 4-methoxybenzoic acid, 25g of a mixture of phosphorus pentoxide and methanesulfonic acid (phosphorus pentoxide to methanesulfonic acid weight ratio is 7:100) are added to a dry three-necked flask with nitrogen, stirred and reacted at a temperature of 60°C for 1 hour, and then the reactants are added to 100mL of ice water and allowed to stand. The resulting precipitate is washed with water, 0.1mol / L NaHCO3, and water in turn, and finally vacuum dried at a temperature of 80°C for 24 hours to obtain 1.43g of yellow powder with a yield of 97%. The reaction formula is as follows:

[0115]

[0116] The H NMR spectrum of the obtained product is as follows Figure 5 As shown, in Experimental Example 1, a 3-acylated indole derivative was obtained with a yield of 97%, and the nitrogen and other positions on the indole ring did not undergo acylation reaction with 4-methoxybenzoic acid (even in the presence of excess 4-methoxybenzoic acid), indicating that the acylation reaction occurred quantitatively and selectively at the 3-position of the indole ring.

[0117] Experimental Example 2

[0118] This experimental example is used to test the performance of the proton exchange membranes obtained in Example 17 and Example 18 at different temperatures. The conductivity of the proton exchange membrane was measured using a PGSTAT302N electrochemical workstation (Metrohm China Ltd.) using a known four-electrode model according to GB / T 20042.3-2009, and the results are shown in Table 1:

[0119] Table 1

[0120] membrane Temperature / ℃ humidity Proton conductivity mS / cm Swelling rate Embodiment 17 30 100% 150 2.5% Embodiment 17 80 100% 288 4.1% Embodiment 18 30 100% 160 3.5% Embodiment 18 80 100% 307 13.8%

[0121] In addition, at a temperature of 80° C., the proton exchange membrane in Example 17 remained intact after being immersed in 3% hydrogen peroxide (containing 2ppm FeSO4) for 3 hours, and the weight of the membrane decreased by less than 1% compared with the initial weight. This shows that the proton exchange membrane provided by the present invention has excellent comprehensive properties such as high conductivity, high swelling resistance, high resistance to free radical oxidation, and has great application prospects in proton exchange membrane fuel cells.

Claims

1. An indole sulfonated monomer, characterized in that: The structure of the indole sulfonated monomer is shown in Formula 1: R1 in formula 1 is -(CH2) n -, n is 3 or 4, G1 is -SO3M; M in -SO3M and -OM in Formula 1 are both selected from any one atom of Li, Na, K or H.

2. A method for preparing an indole sulfonated monomer as claimed in claim 1, characterized in that: The following steps are involved: First, indole-6-carboxylate, alkali metal alkoxide and sultone are mixed for sulfonation reaction, and then an alkaline aqueous solution is added to the sulfonation reaction product for hydrolysis reaction, or an alkaline aqueous solution is added to the sulfonation reaction product for hydrolysis reaction, and then an acidic cation exchange resin is used to perform ion exchange on the hydrolysis reaction product; wherein the sultone is 1,3-propyl sultone or 1,4-butyl sultone.

3. The method for preparing an indole sulfonated monomer according to claim 2, characterized in that: The temperature of the sulfonation reaction is 30 to 100° C., and the reaction time is 2 to 24 hours.

4. An indole sulfonated polymer, characterized in that: The indole sulfonated polymer includes a structural unit as shown in Formula 2: R2 in formula 2 is -(CH2) n -, n is 3 or 4, G2 is -SO3Q, and Q is a cation.

5. The indole sulfonated polymer according to claim 4, characterized in that: The indole sulfonated polymer further includes a structural unit as shown in Formula 3: R3 in the structural unit shown in Formula 3 is selected from -H or a C1-C10 straight-chain alkyl group.

6. The indole sulfonated polymer according to any one of claims 4 to 5, characterized in that: The inherent logarithmic viscosity of the indole sulfonated polymer is 1.0 to 6.0 dL / g; wherein the inherent logarithmic viscosity is measured by the following steps: using 99% pure methanesulfonic acid as a solvent, preparing the indole sulfonated polymer into a solution with a concentration of 0.3 g / 100 mL, and measuring the inherent logarithmic viscosity using an Ubbelohde viscometer at a temperature of 30°C.

7. A method for preparing an indole sulfonated polymer, characterized in that: The following steps are involved: The reaction monomers are polymerized under the catalytic action of phosphorus pentoxide and methanesulfonic acid; The reactive monomer comprises the indole sulfonated monomer as claimed in claim 1.

8. The method for preparing an indole sulfonated polymer according to claim 7, characterized in that: The reactive monomers also include comonomers as shown in Formula 4: R4 in the comonomer represented by Formula 4 is selected from -H or a C1-C10 straight-chain alkyl group.

9. A method for preparing a proton exchange membrane, characterized in that: The following steps are involved: A solution containing the indole sulfonated polymer according to any one of claims 4 to 6 is coated on the surface of a substrate, and the solvent is removed to obtain a proton exchange membrane.

Citation Information

Patent Citations

  • Sulfonated aromatic compound, polyketone with sulfonated aromatic groups and methods for preparing sulfonated aromatic compound and polyketone with sulfonated aromatic groups

    CN103044292A

  • Side chain sulfonated polyketone containing binaphthalene structure and preparation method thereof

    CN104371092A

  • Polybenzole compound having sulfo group and / or phosphono group, resin composition containing same, molded resin, solid polymer electrotyte film, solid electrolyte film / electrode catalyst layer ...

    CN1474844A