A series of maleic anhydride selective hydrogenation catalysts and use method thereof

Through the tandem malic anhydride selective hydrogenation catalyst, the combination of copper-based catalyst and solid base is used to solve the problem of insufficient conversion rate and selectivity of reaction intermediates in the prior art, and efficient γ-butyrolactone synthesis is achieved. Suitable for large-scale production.

CN116272989BActive Publication Date: 2024-11-01LINHAI LIANSHENG CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310168511.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-11-01
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

The existing maleic anhydride selective hydrogenation catalysts have shortcomings in improving the conversion rate of reaction intermediates and GBL selectivity, especially inadequate utilization of hemiacetal catalysts, resulting in low conversion and selectivity.

Method used

The selective hydrogenation catalyst of tandem type is composed of a copper-based catalyst and a solid base through tandem. The copper-based catalyst has a selective hydrogenation effect. The solid base promotes the catalytic conversion of hemiacetals, promotes chemical equilibrium to move to the right, and passes through evaporation. The copper-based catalyst was prepared by ammonia method and mixed with quartz sand to fill the fixed bed reaction device, and the reaction was carried out after reduction using hydrogen.

Benefits of technology

The selectivity and yield of γ-butyrolactone are significantly improved, the hemiacetal conversion rate is promoted, and the efficient γ-butyrolactone synthesis is achieved, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116272989B_ABST
    Figure CN116272989B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of chemical technology, and relates to a series-type maleic anhydride selective hydrogenation catalyst and a method for using the same. The present invention discloses a series-type maleic anhydride selective hydrogenation catalyst, which is composed of a metal catalyst and a solid base in series at a mass ratio of (0.5-5):1, and the metal catalyst includes one or more of a copper-based catalyst and a copper-magnesium-based catalyst; the copper content in the copper-based catalyst is 10-50wt%; the Mg content in the copper-magnesium-based catalyst is 3-20wt%, and the copper content is 28-40wt%. The present invention also discloses a method for using the series-type maleic anhydride selective hydrogenation catalyst, which comprises: mixing the series-type maleic anhydride selective hydrogenation catalyst with quartz sand and filling it into the middle of a reaction tube of a continuous fixed bed reaction device, and fixing the upper and lower ends of the catalyst bed with quartz wool; and then reducing the particle mixed catalyst to a reaction temperature by hydrogen reduction before use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical industry and relates to a series-type maleic anhydride selective hydrogenation catalyst and a use method thereof. Background Art

[0002] γ-Butyrolactone (GBL) is an important C4 chemical intermediate, which is widely used in fine chemicals and pharmaceutical intermediates. Selective hydrogenation of maleic anhydride is one of the most valuable routes for producing GBL. According to the reaction pathway of preparing GBL by hydrogenation of maleic anhydride, succinic anhydride (also known as succinic anhydride) is hydrogenated to generate an important intermediate hemiacetal, which is often ignored in the entire maleic anhydride hydrogenation process. In this process, hemiacetal and its tautomer β-formylpropionic acid are in dynamic equilibrium, but molecules with acyl and hydroxyl (or carboxyl) groups tend to form stable hemiacetals, so the equilibrium is biased towards hemiacetal, while β-formylpropionic acid has high reactivity and is easily hydrogenated, so β-formylpropionic acid is converted into γ-butyrolactone with higher conversion rate and GBL selectivity.

[0003] In order to improve the catalytic activity and GBL selectivity, a large number of literature and patents have reported on catalyst active centers and modulating additives. At present, whether it is the hydrogenation of maleic anhydride to 1,4-butanediol or the dehydrogenation of 1,4-butanediol to produce γ-butyrolactone, the industry usually uses copper-based catalysts; for example, the Chinese patent application text (publication number: CN112742396A) discloses a copper-based silicon-based composite catalyst comprising a copper component, a silicon component and an additive element, which is prepared by a conventional precipitation method, wherein the content of the copper component is 2 to 50 wt% in terms of CuO, and contains common additives such as Na, K, Cs, W, Mn, Re, Ru, Sn, Sb, Bi, La, Ag, Mn, etc., mainly electronic additives and metal oxides, and the mechanism of action of the above additives on chemical equilibrium has not been proposed. The Chinese patent (publication number CN110773174A) introduces a Mg source and uses a coprecipitation method to prepare a precursor with a hydrotalcite structure. The catalyst has a petal-like structure. The coordination of the active component Cu with other metals can effectively prevent the catalyst from sintering or agglomerating during high temperature. It is believed that the auxiliary agent Zn can adjust the acidity and alkalinity of the catalyst. Since the alkaline catalyst can inhibit the dehydration of the catalyst, the formation of by-products tetrahydrofuran and butanol can be eliminated in the dehydration and dehydrogenation reaction of 1,4-butanediol to prepare γ-butyrolactone. However, Zn is a weak Lewis acid and base, which has a small effect on the conversion rate and a weak ability to shift the overall chemical equilibrium to the right.

[0004] At present, the catalysts for the selective hydrogenation of maleic anhydride mainly focus on Cu-based catalysts, additives, and morphology or structure modification. Based on previous literature and patents, there are still important deficiencies in this system: the selective hydrogenation network of maleic anhydride polyunsaturated bonds needs to be refined. If a conversion hemiacetal catalyst can be introduced, the conversion rate of the reaction intermediates can be greatly improved, thereby improving the maleic anhydride conversion rate and the target product GBL selectivity. In summary, the preparation of an active component that can improve the conversion of intermediates is of great significance for the selective hydrogenation of maleic anhydride. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned problems existing in the existing maleic anhydride selective hydrogenation catalyst and propose a tandem maleic anhydride selective hydrogenation catalyst, which can greatly improve the conversion rate of reaction intermediates, thereby improving the maleic anhydride conversion rate and the target product GBL selectivity.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A tandem maleic anhydride selective hydrogenation catalyst, the tandem maleic anhydride selective hydrogenation catalyst is composed of a metal catalyst and a solid base in series at a mass ratio of (0.5-5):1.

[0008] The metal catalyst includes one or more of a copper-based catalyst and a copper-magnesium-based catalyst;

[0009] The copper content of the copper-based catalyst is 10 to 50 wt%;

[0010] The copper-magnesium-based catalyst contains 3-20 wt% Mg and 28-40 wt% copper.

[0011] The metal-based catalyst and the solid base in the serial maleic anhydride selective hydrogenation catalyst of the present invention are connected in series, wherein the metal-based catalyst has the function of selectively hydrogenating C=C double bonds and C=O double bonds; the solid base promotes the catalytic conversion of the reaction intermediate hemiacetal and promotes the chemical equilibrium to move to the right.

[0012] Preferably, the copper content in the copper-based catalyst is 30-40 wt%.

[0013] Preferably, the solid base is one or more of metal oxides, basic molecular sieves, and supported solid base catalysts.

[0014] Further preferably, the metal oxide includes one or more of MgO and CaO; the supported solid base includes one or more of KF / Al2O3 and K2O / Al2O3; and the basic molecular sieve includes one or more of 4A, 5A and 13X.

[0015] Preferably, the copper-based catalyst is prepared from copper salt by an ammonia evaporation method, and the preparation method of the copper-based catalyst comprises: adding a dissolved copper salt solution dropwise to a mixed solution of ammonia water and alkaline silica sol, placing in a constant temperature water bath after aging, heating and evaporating ammonia until the pH value of the solution reaches 7, and obtaining a copper-based catalyst after standing, filtering, drying and calcining.

[0016] Preferably, the preparation method of the copper-magnesium-based catalyst comprises: adding a dissolved mixed solution of copper salt and magnesium salt to a mixed solution of ammonia water and alkaline silica sol, placing it in a constant temperature water bath after aging, heating and evaporating ammonia until the pH value of the solution reaches 7; and preparing the catalyst by standing, filtering, drying and calcining.

[0017] Preferably, the mass ratio of ammonia water to alkaline silica sol in the mixed solution is (1-3):1; the mass ratio of the mixed solution to copper salt solution is 1:(1.5-3).

[0018] More preferably, concentrated aqueous ammonia with a mass content of 20-30% is added during the preparation of the copper-based catalyst and the copper-magnesium-based catalyst.

[0019] Preferably, the aging temperature is 85-95°C, and the aging time is 1-24 hours; the constant temperature water bath temperature is 45-60°C, and the aging time is 5-8 hours.

[0020] Preferably, the temperature of the ammonia evaporation process is 85-95°C.

[0021] Preferably, the calcination process is carried out at a temperature of 300 to 500° C. and for a time of 3 to 24 hours.

[0022] Preferably, the metal catalyst and the solid base are mixed in the form of particles.

[0023] The present invention also discloses a method for using a tandem maleic anhydride selective hydrogenation catalyst, which comprises: mixing the tandem maleic anhydride selective hydrogenation catalyst with quartz sand and filling the mixture into the middle of a reaction tube of a continuous fixed bed reaction device, fixing the upper and lower ends of the catalyst bed with quartz wool; and then reducing the particle mixed catalyst with hydrogen and lowering it to the reaction temperature before use.

[0024] The tandem maleic anhydride selective hydrogenation catalyst of the present invention promotes the conversion of hemiacetal to β-formylpropionic acid, promotes the chemical equilibrium to move to the right, significantly improves the selectivity of γ-butyrolactone (GBL), and improves the yield of γ-butyrolactone (GBL). In addition, the mixed catalyst needs to be reduced with hydrogen after filling before it can be used in the reaction process of preparing γ-butyrolactone (GBL), because the maleic anhydride hydrogenation active component requires a low-valent metal.

[0025] Preferably, the mass ratio of the tandem maleic anhydride selective hydrogenation catalyst to quartz sand is 1:(1-3).

[0026] Preferably, the temperature of the hydrogen reduction process is 280-350° C. and the time is 5-7 hours.

[0027] Preferably, the filling process includes one or more of a physical mixing method, a powder mixing method, and a two-stage method.

[0028] Preferably, the particle size of the tandem maleic anhydride selective hydrogenation catalyst is 20 to 40 meshes; the particle size of the quartz sand is 20 to 40 meshes.

[0029] Preferably, maleic anhydride is pumped into the continuous fixed bed reaction device by a high-pressure plunger pump, and hydrogen is input through a total hydrogen pipeline.

[0030] Preferably, after the method of using the serial maleic anhydride selective hydrogenation catalyst is adopted, the maleic anhydride conversion rate is 80-100%, and the gamma-butyrolactone (GBL) selectivity is 60-95%.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The tandem maleic anhydride selective hydrogenation catalyst of the present invention is composed of a metal-based catalyst and a solid base, which promotes the right shift of the chemical equilibrium and significantly improves the selectivity of γ-butyrolactone; promotes the conversion rate of hemiacetal to β-formylpropionic acid, and β-formylpropionic acid is easy to hydrogenate, and through the dehydration step, the high-yield synthesis of the final product γ-butyrolactone is achieved.

[0033] 2. The metal-based catalyst in the tandem maleic anhydride selective hydrogenation catalyst of the present invention is prepared from copper salt by an ammonia evaporation method, and an auxiliary agent is added during the temperature-raising ammonia evaporation process to promote the rapid conversion of the intermediate product.

[0034] 3. The use method of the tandem maleic anhydride selective hydrogenation catalyst of the present invention is simple and easy to operate, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the XRD spectrum of the copper-based catalyst prepared in Example 1 of the present invention.

[0036] Figure 2 The figure is a reaction pathway diagram of preparing γ-butyrolactone by hydrogenating maleic anhydride according to the present invention.

[0037] Figure 3 This is the XRD spectrum of the 5A solid base catalyst used in Example 4 of the present invention.

[0038] Figure 4 This is the XRD spectrum of the 13X solid base catalyst used in Example 5 of the present invention. DETAILED DESCRIPTION

[0039] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0040] The alkaline molecular sieve and metal oxide used in the present invention are commercially available materials;

[0041] Basic molecular sieves include 3A, 4A, 5A, and 13X molecular sieves;

[0042] The metal oxides include MgO and CaO.

[0043] Example 1

[0044] Preparation of copper-based catalysts:

[0045] The copper-based catalyst (Cu-SiO2) was prepared by the ammonia evaporation method.

[0046] Weigh 11.4g of Cu(NO3)2·3H2O, add 22.8g of deionized water to prepare copper nitrate solution, then add 25% ammonia water, adjust the pH value to 11.0 to form a copper ammonia solution. Then weigh 13.6g of alkaline silica sol (SiO2, mass fraction 30%) as a silicon source and add it dropwise to the copper ammonia solution. After stirring at room temperature for 4h, evaporate ammonia at 90℃; then age at 90℃ for 12h, filter, wash and dry at 120℃ overnight, roast at 350℃ for 6h, and press into tablets to 20-40 mesh, with a Cu content of 30wt%.

[0047] Figure 1 is the XRD spectrum of the prepared copper-based catalyst.

[0048] Preparation of KF / Al2O3 solid base catalyst:

[0049] Dissolve 10 g of KF in 30 mL of anhydrous ethanol, add support Al2O3 (10 g) dried at 200°C, stir at 60°C for 3 h, and remove the ethanol solvent; after vacuum drying at 120°C, place in a muffle furnace and calcine at 500°C for 6 h to obtain a supported KF / Al2O3 solid base catalyst.

[0050] Synthesis of γ-butyrolactone:

[0051] In this embodiment, a tandem maleic anhydride selective hydrogenation catalyst is used to prepare γ-butyrolactone, which relates to a method for using the tandem maleic anhydride selective hydrogenation catalyst.

[0052] Figure 2 The figure is a reaction pathway diagram of preparing γ-butyrolactone by hydrogenating maleic anhydride according to the present invention.

[0053] The specific method of use includes: mixing copper-based catalyst, solid base catalyst (KF / Al2O3) (30 mesh), and quartz sand (30 mesh) and filling them into the middle of the reaction tube of the continuous fixed bed reaction device, the mass ratio of copper-based catalyst: solid base catalyst is 1:1, the mass ratio of tandem maleic anhydride selective hydrogenation catalyst and quartz sand is 2:1, and the upper and lower ends of the catalyst bed are fixed with quartz wool. Then, the mixed catalyst is reduced at 300°C for 6 hours by hydrogen input through the total hydrogen pipeline, and then lowered to the reaction temperature; maleic anhydride is pumped in by a high-pressure plunger pump.

[0054] The reaction was carried out at a temperature of 240°C, a pressure of 0.5 MPa, a space velocity of 0.2, and a hydrogen anhydride ratio of 80 to obtain γ-butyrolactone. The specific results are shown in Table 1.

[0055] Example 2

[0056] The tandem maleic anhydride selective hydrogenation catalyst of this embodiment is a copper-magnesium based catalyst.

[0057] The CuMg-SiO2 catalyst containing Mg as an additive was prepared by ammonia evaporation method.

[0058] Weigh 11.4g of Cu(NO3)2·3H2O and 2.6g of Mg(NO3)2·6H2O, add 28g of deionized water to prepare a copper nitrate solution, then add 25% ammonia water, adjust the pH value to 11.0 to form a copper ammonia solution. Weigh 11.7g of alkaline silica sol (SiO2, mass fraction 30%) as a silicon source and add it dropwise to the copper ammonia solution. After stirring at room temperature for 4h, evaporate ammonia at 90℃, then age at 90℃ for 12h, filter, wash and dry at 120℃ overnight, roast at 350℃ for 6h, and press into tablets to 20-40 mesh. The Mg content is 5wt%, and the Cu content is 30wt%.

[0059] Synthesis of γ-butyrolactone:

[0060] In this embodiment, a tandem maleic anhydride selective hydrogenation catalyst is used to prepare γ-butyrolactone, which relates to a method for using the tandem maleic anhydride selective hydrogenation catalyst.

[0061] Specifically, the CuMg-SiO2 catalyst (30 mesh), solid base catalyst, and quartz sand (30 mesh) are mixed and filled into the middle of the reaction tube of the continuous fixed bed reaction device, the mass ratio of the serial maleic anhydride selective hydrogenation catalyst and the quartz sand is 2:1, and the upper and lower ends of the catalyst bed are fixed with quartz wool. Then, the mixed catalyst is reduced at 300°C for 6 hours by hydrogen input through the total hydrogen pipeline, and then lowered to the reaction temperature; maleic anhydride is pumped in by a high-pressure plunger pump.

[0062] The reaction was carried out at a temperature of 240°C, a pressure of 0.5 MPa, a space velocity of 0.2, and a hydrogen anhydride ratio of 80 to obtain γ-butyrolactone. The specific results are shown in Table 1.

[0063] Example 3

[0064] Compared with Example 1, the difference is that the solid base is 4A molecular sieve, and the mass ratio of the copper-based catalyst and the solid base catalyst in the tandem maleic anhydride selective hydrogenation catalyst is 1:1.

[0065] Example 4

[0066] Compared with Example 1, the difference is that the solid base is 5A molecular sieve, and the mass ratio of the copper-based catalyst and the solid base catalyst in the tandem maleic anhydride selective hydrogenation catalyst is 1:1.

[0067] Figure 3 This is the XRD spectrum of 5A molecular sieve.

[0068] Example 5

[0069] Compared with Example 1, the difference is that the solid base is 13X molecular sieve, and the mass ratio of the copper-based catalyst and the solid base catalyst in the tandem maleic anhydride selective hydrogenation catalyst is 1:1.

[0070] Figure 4 This is the XRD spectrum of 13X molecular sieve.

[0071] Example 6

[0072] Compared with Example 1, the difference is that the tandem maleic anhydride selective hydrogenation catalyst is composed of a mixture of a copper-based catalyst (Cu-SiO2) and solid base MgO particles, so that the Mg content is 5wt% and the Cu content is 30wt%.

[0073] Example 7

[0074] Compared with Example 6, the difference is that the ratio of the copper-based catalyst (Cu-SiO2) and the solid base MgO is changed so that the content of Mg is 7wt% and the content of Cu is 30wt%.

[0075] Example 8

[0076] Compared with Example 6, the difference is that the ratio of the copper-based catalyst (Cu-SiO2) and the solid base MgO is changed so that the content of Mg is 25wt% and the content of Cu is 30wt%.

[0077] Example 9

[0078] Compared with Example 1, the difference is that the tandem maleic anhydride selective hydrogenation catalyst is composed of a mixture of Cu-SiO2, MgO, and 13A molecular sieve particles in a mass ratio of 1:0.5:0.5.

[0079] Comparative Example 1

[0080] Compared with Example 1, the difference is that no solid base is added, and the tandem maleic anhydride selective hydrogenation catalyst is only a copper-based catalyst.

[0081] Comparative Example 2

[0082] Compared with Example 1, the difference is that no solid base is added, and the tandem maleic anhydride selective hydrogenation catalyst is only a copper-based catalyst; and the amount of copper salt added is adjusted so that the Cu content in the copper-based catalyst is 40wt%.

[0083] Comparative Example 3

[0084] Compared with Example 1, the difference is that the total mass of the copper-based catalyst and the solid base in the tandem maleic anhydride selective hydrogenation catalyst remains unchanged, and the mass ratio of the copper-based catalyst to the solid base is 0.4:1.

[0085] Comparative Example 4

[0086] Compared with Example 1, the difference is that the total mass of the copper-based catalyst and the solid base in the tandem maleic anhydride selective hydrogenation catalyst remains unchanged, and the mass ratio of the copper-based catalyst to the solid base is 5.2:1.

[0087] Table 1. Parameters of tandem maleic anhydride selective hydrogenation catalyst and performance data for preparing γ-butyrolactone

[0088]

[0089] In summary, the tandem maleic anhydride selective hydrogenation catalyst of the present invention is composed of a copper-based catalyst and a solid base, which promotes the right shift of the chemical equilibrium and significantly improves the selectivity of γ-butyrolactone; promotes the conversion rate of hemiacetal to β-formylpropionic acid, and β-formylpropionic acid is easy to hydrogenate, and through the dehydration step, the high-yield synthesis of the final product γ-butyrolactone is achieved.

[0090] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A tandem maleic anhydride selective hydrogenation catalyst, characterized in that: The tandem maleic anhydride selective hydrogenation catalyst is composed of a metal catalyst and a solid base connected in series at a mass ratio of (0.5-5):

1. The metal catalyst includes one or more of a copper-based catalyst and a copper-magnesium-based catalyst; the solid base is one or more of a metal oxide, a molecular sieve and a supported solid base catalyst; the metal oxide includes one or more of MgO and CaO; the supported solid base includes one or more of KF / Al2O3 and K2O / Al2O3; the molecular sieve includes one or more of 4A, 5A and 13X; The copper content in the copper-based catalyst is 10-50wt%; The copper-magnesium-based catalyst has a Mg content of 3-20 wt % and a copper content of 28-40 wt %.

2. The tandem maleic anhydride selective hydrogenation catalyst according to claim 1, characterized in that: The copper-based catalyst is prepared from copper salt by an ammonia evaporation method. The preparation method of the copper-based catalyst comprises: dropping dissolved copper salt into a mixed solution of ammonia water and alkaline silica sol, placing in a constant temperature water bath after aging, heating and evaporating ammonia until the pH value of the solution reaches 7, and obtaining the copper-based catalyst after standing, filtering, drying and roasting.

3. The tandem maleic anhydride selective hydrogenation catalyst according to claim 1, characterized in that: The preparation method of the copper-magnesium-based catalyst comprises: dropping a dissolved mixed solution of copper salt and magnesium salt into a mixed solution of ammonia water and alkaline silica sol, placing in a constant temperature water bath after aging, heating and evaporating ammonia until the pH value of the solution reaches 7; and preparing the catalyst by standing, filtering, drying and roasting.

4. The tandem maleic anhydride selective hydrogenation catalyst according to claim 2 or 3, characterized in that: The aging temperature is 85-95° C., and the aging time is 1-24 hours; the constant temperature water bath temperature is 45-60° C., and the aging time is 5-8 hours.

5. The tandem maleic anhydride selective hydrogenation catalyst according to claim 2 or 3, characterized in that: The calcination process is carried out at a temperature of 300-500°C and a time of 3-24 hours.

6. The tandem maleic anhydride selective hydrogenation catalyst according to claim 2 or 3, characterized in that: The mass ratio of ammonia water to alkaline silica sol in the mixed solution is (1-3):

1.

7. A method for using a tandem maleic anhydride selective hydrogenation catalyst, characterized in that: The method of use comprises: mixing the serial maleic anhydride selective hydrogenation catalyst and quartz sand as claimed in claim 1 and filling the mixture into the middle of the reaction tube of the continuous fixed bed reaction device, fixing the upper and lower ends of the catalyst bed with quartz wool; and then reducing the mixed catalyst with hydrogen and lowering it to the reaction temperature before use.

8. The method for using the tandem maleic anhydride selective hydrogenation catalyst according to claim 7, characterized in that: The temperature of the hydrogen reduction process is 280~350℃ and the time is 5~7h.

9. The method for using the tandem maleic anhydride selective hydrogenation catalyst according to claim 7, characterized in that: The mass ratio of the tandem maleic anhydride selective hydrogenation catalyst to quartz sand is 1:(1-3).

10. The method for using the tandem maleic anhydride selective hydrogenation catalyst according to claim 7, characterized in that: The particle size of the tandem maleic anhydride selective hydrogenation catalyst is 20-40 meshes; the particle size of the quartz sand is 20-40 meshes.

11. The method for using the tandem maleic anhydride selective hydrogenation catalyst according to claim 7, characterized in that: After the method for using the serial maleic anhydride selective hydrogenation catalyst is adopted, the maleic anhydride conversion rate is 80-100%, and the gamma-butyrolactone (GBL) selectivity is 60-95%.