Preparation and application of a carbon-based bimetallic nanocluster catalyst

By using impregnation reduction method on porous carbon-based support, the problem of large size and low activity of catalyst particles in the prior art is solved, and efficient CO2 reduction performance and green process are achieved, which is suitable for CO2 reduction reaction.

CN116273118BActive Publication Date: 2024-11-15XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310181822.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-11-15
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

The prior art is difficult to prepare Pt-Ru bimetallic nanocluster catalysts with high catalytic activity, and commonly used methods involve high toxic organic solvents and high cost rare earth elements, which limits their wide application.

Method used

The metal particles were loaded on a porous carbon-based support by impregnation reduction method to prepare a carbon-based bimetallic nanocluster catalyst. Through ultrasonic stirring and reflux processes, the homogeneity and dispersion of the metal clusters were ensured, and the conditions were successfully carried out under mild conditions. Prepare nanoclusters.

Benefits of technology

It has achieved rapid, simple and high success rate preparation of carbon-based bimetallic nanocluster catalysts, with high catalytic activity, especially in CO2 reduction reaction, and the process is in line with the concept of green development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116273118B_ABST
    Figure CN116273118B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation and application of a carbon-based bimetallic nanocluster catalyst, step 1: adding RuCl3.3H2O to deionized water, ultrasonically stirring, and obtaining a uniformly dispersed solution; step 2: adding the prepared porous carbon-based carrier to the dispersed solution in step 1, and continuing ultrasonic stirring; step 3: adding H2PtCl6.6H2O to the dispersed solution in step 2, and then continuing stirring; step 4: taking potassium borohydride powder, adding it to deionized water, ultrasonically obtaining a uniformly dispersed solution; step 5: pouring the solution in step 3 into a three-necked flask, and placing the three-necked flask in an oil bath; step 6: adding the prepared solution in step 4 to the three-necked flask in step 5, and assembling a reflux pipe to reflux it; step 7: filtering and washing the solution in step 6, and then freeze-drying, removing the remaining solvent molecules, and obtaining a carbon-based bimetallic nanocluster catalyst. The invention has the characteristics of being fast, simple and having a high success rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalyst preparation and application, and specifically relates to the preparation and application of a carbon-based bimetallic nanocluster catalyst. Background Art

[0002] Nanoclusters are relatively stable aggregates composed of several or even 10 atoms or molecules bound together by physical or chemical effects. Due to their small size, large specific surface area, and the unsaturated and non-directional bonding of surface atoms, nanoclusters have some unique properties: size effect. For small-sized clusters, due to quantum effects, metals that are inert in the bulk phase show outstanding catalytic properties at the nanoscale. In addition, the stability, electronic structure and thermodynamic properties of the clusters are all affected by the size effect. Surface effect. The coordination numbers of many atoms on the surface of nanoclusters, such as the atoms on the vertices, edges and faces, cannot reach saturation. This unsaturated coordination can easily produce active centers. In addition, nanoclusters have a large specific surface area, so the cluster surface will show high catalytic activity.

[0003] At present, Martin et al. have synthesized a Pt-Ru bimetallic nanoparticle catalyst using a hydrothermal method (a hydrothermal synthesis method and application of Pt-Ru bimetallic nanoparticles: CN201410680749.5[P].2015-04-08.); Liang Xin et al. introduced rare earth combined with solvent thermal synthesis technology into the platinum ruthenium system to prepare a platinum ruthenium nanoparticle catalyst (a preparation method of platinum ruthenium nanoparticles modified with rare earth elements: CN202210224723.4[P].2022-06-28.) Although the above method can synthesize Pt-Ru bimetallic nanoparticle catalysts, the overall size of the catalyst particles is relatively large (greater than 2nm), and it cannot have the advantages of large specific surface area of ​​nanoclusters and high catalytic activity. At the same time, the above preparation method involves highly toxic organic solvents such as DMF and relatively high-cost rare earth elements, which is not conducive to large-scale promotion and application. Summary of the invention

[0004] In order to overcome the defects of the above prior art, the purpose of the present invention is to provide a preparation and application of a carbon-based bimetallic nanocluster catalyst, which uses an impregnation reduction method to load metal particles on a porous carbon-based carrier to prepare a carbon-based bimetallic nanocluster catalyst, with a metal particle size of less than 2nm, while ensuring that the metal clusters have a high uniformity and dispersion. The method is fast, simple and has a high success rate.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A carbon-based bimetallic nanocluster catalyst, wherein the carbon-based bimetallic nanocluster catalyst is: Ptnanoclusters-Ru nanoclusters (PtNCs-RuNCs / PDMC), wherein the metal nanoclusters are loaded on heteroatom-doped nanoporous carbon spheres, wherein the metal Pt and the metal Ru exist in different proportions, and the porous carbon spheres are polyaniline-derived mesoporous carbon spheres (PDMC) doped with heteroatoms such as N and O;

[0007] The chemical composition (wt.%) of the carbon-based bimetallic nanocluster catalyst (PtNCs-RuNCs / PDMC) is: Pt: 2-5wt.%; Ru: 30-35wt.%; C: 55-65wt.%, and the sum of N, O and S contents: 3-5wt.%.

[0008] A method for preparing a carbon-based bimetallic nanocluster catalyst comprises the following steps:

[0009] Step 1: Add RuCl3.3H2O to deionized water and perform ultrasonic stirring to obtain a uniformly dispersed solution;

[0010] Step 2: adding the prepared N,O heteroatom-doped mesoporous carbon spheres derived from polyaniline to the dispersed solution in step 1, and continuing ultrasonic stirring;

[0011] Step 3: Add H2PtCl6.6H2O to the dispersion in step 2, and continue stirring;

[0012] Step 4: Take potassium borohydride powder, add it to deionized water and ultrasonicate to obtain a uniformly dispersed solution;

[0013] Step 5: Pour the solution in step 3 into a three-necked flask, and place the three-necked flask in an oil bath;

[0014] Step 6: Add the solution prepared in step 4 to the three-necked flask in step 5, and assemble the reflux tube to allow it to reflux;

[0015] Step 7: The solution of step 6 is filtered and washed, and then freeze-dried to remove the remaining solvent molecules to obtain a carbon-based bimetallic nanocluster catalyst.

[0016] The N,O heteroatom-doped mesoporous carbon spheres derived from polyaniline in step 2 are uniform porous carbon-based carriers prepared by aniline polymerization and silicon template method, with uniform pore size and high integration. Among them, the porous carbon-based carrier can also be synthesized by other methods, and the pore size prepared by the silicon template method is uniform and highly integrated.

[0017] The RuCl3.3H2O and H2PtCl6.6H2O involved in step 1 and step 3 contain two metal elements, Ru and Pt, respectively;

[0018] Among them, the metal elements that can be used in the preparation method include any two of Ru, Pt, Ni, Pd, Rh, Ir, Cu, Zn, and Ag.

[0019] In step 1 and step 2, ultrasonic stirring is performed for 30 minutes, and in step 3, stirring is performed for 12 hours.

[0020] In step 5, the temperature of the oil bath is set to 70-90° C. to facilitate reflux operation.

[0021] In step 6, the reflux tube is assembled and refluxed at 70-90° C. for 1-4 hours to fully reduce the catalyst; wherein the solvent is water, and therefore the reflux operation temperature cannot be higher than 100° C. The purpose of the reflux operation is to enable the catalyst to be reduced more fully.

[0022] In step 7, freeze drying is performed for 5-20 hours; after filtration and washing, there is still water, so drying is required, and freeze drying has a better effect.

[0023] The chemical composition (wt.%) of the carbon-based bimetallic nanocluster catalyst (PtNCs-RuNCs / PDMC) is: Pt: 2-5wt.%; Ru: 30-35wt.%; C: 55-65wt.%, and the sum of N, O and S content: 3-5wt.%. The mass ratios of the porous carbon-based carrier, ruthenium chloride trihydrate, chloroplatinic acid and potassium borohydride during the preparation of the catalyst PtNCs-RuNCs / PDMC are: 43-60: 36-50: 4-10: 135-150. In the preparation process, since the solvent is water, elements such as K are soluble in water, so they are washed away during the filtration and washing.

[0024] The carbon-based bimetallic nanocluster catalyst is used for CO2 reduction.

[0025] Beneficial effects of the present invention:

[0026] 1. The present invention discloses a method for loading metal particles on a porous carbon-based carrier by an impregnation reduction method, which is a fast, simple and highly successful method for preparing a carbon-based bimetallic nanocluster catalyst.

[0027] 2. The present invention can prepare carbon-based bimetallic nanocluster catalysts while ensuring that the metal clusters have high uniformity and dispersion.

[0028] 3. Two metal atoms were introduced onto the porous carbon-based carrier and two metal clusters were successfully prepared, further improving the catalytic ability between the clusters.

[0029] 4. The preparation process is simple and the atomic utilization rate is high, which is in line with the concept of green development.

[0030] 5. The reaction conditions are mild, and nanocluster catalysts can be successfully prepared without high temperature and high pressure (the reaction temperature is lower than 100°C and no external pressure is required) or harsh external conditions.

[0031] 6. The catalyst of the present invention has good catalytic performance for CO2 reduction.

[0032] In the present invention, the structural characteristics of the porous carbon carrier and the uniform distribution of components such as N and O can effectively pin and adsorb the precursor, and the size growth of Ru and Pt clusters is controlled by controlling parameters such as metal reduction temperature, reducing agent concentration, and time. The obtained diatomic sizes are all within 2nm and are highly dispersed.

[0033] The structural characteristics of the catalyst of this invention are also as follows: its Ru content is as high as 30%, but it is still highly dispersed and its size is less than 2nm; Pt and Ru clusters are evenly distributed on the surface of the carbon carrier and its pore size, and are not encapsulated therein. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic flow chart of a method for preparing a bimetallic cluster catalyst on a porous carbon-based carrier according to an embodiment of the present invention.

[0035] Figure 2 This is the SEM (scale: 1 um) of the catalyst PtNCs-RuNCs / PDMC prepared in Example 1 of the present invention.

[0036] Figure 3 This is the TEM image of the catalyst PtNCs-RuNCst / PDMC prepared in Example 1 of the present invention (scale: 10 nm).

[0037] Figure 4 It is a particle size statistical histogram of the catalyst PtNCs-RuNCs / PDMC prepared in Example 1 of the present invention.

[0038] Figure 5 Elemental energy spectrum of the catalyst PtNCs-RuNCs / PDMC prepared in Example 1 of the present invention.

[0039] Figure 6 Methane production diagram of the catalyst PtNCs-RuNCs / PDMC prepared in Example 1 of the present invention for CO2 reduction.

[0040] Figure 7Discharge curve of the catalyst PtNCs-RuNCs / PDMC prepared in Example 1 of the present invention for CO2 reduction. DETAILED DESCRIPTION

[0041] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0042] CO2 molecules have good thermodynamic stability, and the C=O dissociation energy is as high as 750kJ / mol, far exceeding other chemical bonds such as CH (430Kj / mol) and CC (336kJ / mol), which leads to difficulty in adsorption activation and slow kinetic reaction. Therefore, the occurrence of CO2 reduction reaction (CO2RR) reaction first requires the input of sufficient energy to promote the dissociation of chemical bonds before further reaction can generate carbon compounds with economic value. Cluster catalysts have excellent catalytic performance and are very beneficial to CO2 reduction. Therefore, this application invents a supported dual cluster catalyst and uses it in CO2 reduction.

[0043] A method for preparing a carbon-based bimetallic nanocluster catalyst of the present invention comprises the following steps:

[0044] (1) Add 26 mg to 65 mg of ruthenium chloride trihydrate particles to 13 to 39 ml of deionized water, and sonicate the solution for 5 to 20 min and stir it magnetically for 15 to 45 min.

[0045] (2) Add 42-60 mg of the carbon-based support prepared by aniline polymerization to the dispersion of step (1), then continue ultrasonication for 5-20 min and magnetic stirring for 10-20 min, and repeat twice.

[0046] (3) The concentration of H3PtCl6 solution is 15-25mmol / L. Take 0.4-1.4ml of the solution and add it to step (2), and then stir it magnetically for 5-20h.

[0047] (4) Pour the dispersion obtained in step (3) into a three-necked flask, place the three-necked flask in an oil bath, and heat the oil bath to 70-90°C.

[0048] (5) The concentration of KBH4 solution is 30-35 mmol / L. Take 2-4 ml of the solution and add it to a three-necked flask.

[0049] (6) Maintain the temperature of the oil bath at 70-90°C and reflux for 1-4 hours.

[0050] (7) The solution after confluence in step (6) is filtered, first washed three times with deionized water, and finally washed once with anhydrous ethanol.

[0051] (8) Place the sample filtered in step (7) in a freeze dryer and set the temperature to -68--48°C for freeze drying for 5-20 hours.

[0052] (9) Take out the catalyst treated in step (8), grind and weigh it, and finally seal it for storage.

[0053] In the embodiment of the present invention, the amount of ruthenium chloride trihydrate is 0.1mmol-0.25mmol, and the mass is 26mg-65mg.

[0054] In the embodiment of the present invention, the porous carbon-based carrier is a porous carbon-based carrier prepared by the aniline polymerization silicon template method, and the usage amount is 45-60 mg, and is not limited to the porous carbon-based carrier prepared by the aniline polymerization silicon template method.

[0055] In the embodiment of the present invention, the concentration of the chloroplatinic acid solution is 0.15-0.25 mmol / L, and the usage is 0.4-1.4 ml.

[0056] In the embodiment of the present invention, the concentration of potassium borohydride is 30mmol / L-35mmol / L, and the usage is 2-4ml.

[0057] In the embodiment of the present invention, the reflux temperature is 70-90° C., and the reflux time is 1-4 h.

[0058] In the embodiment of the present invention, the obtained metal catalyst particles are washed three times with deionized water, washed once with anhydrous ethanol, and then freeze-dried. The freeze-drying temperature is between minus 65°C and minus 50°C. The target catalyst is obtained after freeze-drying for 5-20 hours.

[0059] The method implemented by the present invention loads a bimetallic catalyst on a porous carbon-based carrier and reduces it to make the metal particles grow into nanocluster particles. The impregnation reduction method is adopted, which not only has a very simple process flow but also can ensure the uniformity and dispersion of the bimetallic clusters.

[0060] Example 1

[0061] An impregnation reduction method according to an embodiment of the present invention loads bimetallic particles on a porous carbon-based carrier and ensures that metal atoms are reduced to cluster particles. The specific steps include:

[0062] 43 mg of ruthenium chloride trihydrate particles were added to 25 ml of deionized water, and the mixed solution was ultrasonicated for 15 minutes and magnetically stirred for 30 minutes. After the solution was completely dispersed, 51 mg of porous carbon-based carrier was added, and then ultrasonicated for 15 minutes and magnetically stirred for 15 minutes. After repeating this process twice, 0.7 ml of 19.03 mmol / L H3PtCl6 aqueous solution was added to the above solution, and finally magnetically stirred for 12 hours.

[0063] Pour the stirred dispersion into a three-necked flask, place the three-necked flask in an oil bath, and heat it to 80°C. Dissolve 143.13 mg of KBH4 in 2.687 g of deionized water, add it to the three-necked flask after ultrasonic dissolution, and finally reflux at 80°C for 2 hours. Then filter and wash the refluxed solution, first wash it three times with deionized water, and then wash it once with anhydrous ethanol. After the filtration and washing are completed, set the freeze dryer temperature to -68°C and freeze-dry for 12 hours. Take out the dried catalyst, grind and weigh it, and finally seal it for storage.

[0064] Example 2

[0065] 43 mg of ruthenium chloride trihydrate particles were added to 25 ml of deionized water, and the mixed solution was ultrasonicated for 15 minutes and magnetically stirred for 30 minutes. After the solution was completely dispersed, 51 mg of porous carbon-based carrier was added, and then ultrasonicated for 15 minutes and magnetically stirred for 15 minutes. After repeating this twice, 0.4 ml of 19.03 mmol / L H3PtCl6 aqueous solution was added to the above solution. Finally, it was magnetically stirred for 12 hours.

[0066] Pour the stirred dispersion into a three-necked flask, place the three-necked flask in an oil bath, and heat it to 80°C. Dissolve 143.13 mg of KBH4 in 2.687 g of deionized water, add it to the three-necked flask after ultrasonic dissolution, and finally reflux at 80°C for 2 hours. Then filter and wash the refluxed solution, first wash it three times with deionized water, and then wash it once with anhydrous ethanol. After the suction filtration and washing are completed, set the freeze dryer temperature to -68°C, and then freeze-dry for 12 hours. Take out the dried catalyst, grind and weigh it, and finally seal it for storage.

[0067] Example 3

[0068] 43 mg of ruthenium chloride trihydrate particles were added to 25 ml of deionized water, and the mixed solution was ultrasonicated for 15 minutes and magnetically stirred for 30 minutes. After the solution was completely dispersed, 51 mg of porous carbon-based carrier was added, and then ultrasonicated for 15 minutes and magnetically stirred for 15 minutes. After repeating this process twice, 1.0 ml of 19.03 mmol / L H3PtCl6 aqueous solution was added to the above solution. Finally, it was magnetically stirred for 12 hours.

[0069] Pour the stirred dispersion into a three-necked flask, place the three-necked flask in an oil bath, and heat it to 80°C. Dissolve 143.13 mg of KBH4 in 2.687 g of deionized water, add it to the three-necked flask after ultrasonic dissolution, and finally reflux at 80°C for 2 hours. Then filter and wash the refluxed solution, first wash it three times with deionized water, and then wash it once with anhydrous ethanol. After the suction filtration and washing are completed, set the freeze dryer temperature to -68°C, and then freeze-dry for 12 hours. Take out the dried catalyst, grind and weigh it, and finally seal it for storage.

[0070] Example 4

[0071] 43 mg of ruthenium chloride trihydrate particles were added to 25 ml of deionized water, and the mixed solution was ultrasonicated for 15 minutes and magnetically stirred for 30 minutes. After the solution was completely dispersed, 51 mg of porous carbon-based carrier was added, and then ultrasonicated for 15 minutes and magnetically stirred for 15 minutes. After repeating this process twice, the mixture was magnetically stirred for 12 hours.

[0072] Pour the stirred dispersion into a three-necked flask, place the three-necked flask in an oil bath, and heat it to 80°C. Dissolve 130 mg of KBH4 in 2.687 g of deionized water, add it to the three-necked flask after ultrasonic dissolution, and finally reflux at 80°C for 2 hours. Then filter and wash the refluxed solution, first wash it three times with deionized water, and then wash it once with anhydrous ethanol. After the filtration and washing are completed, set the freeze dryer temperature to -68°C, and then freeze-dry for 12 hours. Take out the dried catalyst, grind and weigh it, and finally seal it for storage.

[0073] Example 5

[0074] 43 mg of ruthenium chloride trihydrate particles were added to 25 ml of deionized water, and the mixed solution was ultrasonicated for 15 minutes and magnetically stirred for 30 minutes. After the solution was completely dispersed, 51 mg of porous carbon-based carrier was added, and then ultrasonicated for 15 minutes and magnetically stirred for 15 minutes. After repeating this process twice, 1 ml of 19.03 mmol of nickel chloride solution was added, and then magnetically stirred for 12 hours.

[0075] Pour the stirred dispersion into a three-necked flask, place the three-necked flask in an oil bath, and heat it to 80°C. Dissolve 143 mg of KBH4 in 2.687 g of deionized water, add it to the three-necked flask after ultrasonic dissolution, and finally reflux at 80°C for 2 hours. Then filter and wash the refluxed solution, first wash it three times with deionized water, and finally wash it once with anhydrous ethanol. After the filtration and washing are completed, set the freeze dryer temperature to -68°C, and then freeze-dry for 12 hours. Take out the dried catalyst, grind and weigh it, and finally seal it for storage.

[0076] The present invention uses an impregnation reduction method to load metal particles on a porous carbon-based carrier, which is a fast, simple and highly successful method for preparing a supported cluster catalyst. The present invention not only has a very simple process flow, but also can ensure the uniformity and dispersion of the bimetallic clusters, thereby further improving the catalytic performance of the catalyst and showing good CO2 reduction performance.

[0077] like Figure 1 As shown: Pt and Ru elements are loaded on a porous carbon-based support and reduced by KBH4 solution;

[0078] like Figure 2 As shown: The main structure of the catalyst PtNCs-RuNCs / PDMC is porous carbon spheres with uniform size and shape;

[0079] like Figure 3 As shown: the particles of the catalyst PtNCs-RuNCs / PDMC are evenly distributed and have similar sizes;

[0080] like Figure 4 As shown: The average size of the catalyst PtNCs-RuNCs / PDMC particles is 1.68nm, which belongs to the range of nanoclusters, indicating that the bimetallic nanocluster catalyst was successfully prepared;

[0081] like Figure 5 As shown: Pt, Ru, C, N, O, and S elements exist in the catalyst PtNCs-RuNCs / PDMC

[0082] like Figure 6 As shown: The catalyst PtNCs-RuNCs / PDMC was used for CO2 reduction, and the CH4 production was the highest at 170°C, reaching 220.8ppm.

[0083] like Figure 7 As shown: The catalyst PtNCs-RuNCs / PDMC is used for CO2 reduction, and the current density is the highest at 170℃, reaching 188.9Am -2 .

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a carbon-based bimetallic nanocluster catalyst, characterized in that: The steps include: Step 1: Add RuCl3.3H2O to deionized water and perform ultrasonic stirring to obtain a uniformly dispersed solution; Step 2: adding the prepared N,O heteroatom-doped mesoporous carbon spheres derived from polyaniline to the dispersed solution in step 1, and continuing ultrasonic stirring to obtain a dispersed solution; Step 3: Add H2PtCl6.6H2O to the dispersion in step 2, and continue stirring; Step 4: Take potassium borohydride powder, add it to deionized water and ultrasonicate to obtain a uniformly dispersed solution; Step 5: Pour the solution in step 3 into a three-necked flask, and place the three-necked flask in an oil bath; Step 6: Add the solution prepared in step 4 to the three-necked flask in step 5, and assemble the reflux tube to allow it to reflux; Step 7: The solution in step 6 is filtered and washed, and then freeze-dried to remove the remaining solvent molecules to obtain a carbon-based bimetallic nanocluster catalyst; The carbon-based bimetallic nanocluster catalyst is: PtNCs-RuNCs / PDMC, the metal nanoclusters are supported on heteroatom-doped nanoporous carbon spheres, wherein metal Pt and metal Ru exist in different proportions, and the porous carbon spheres are polyaniline-derived N,O heteroatom-doped mesoporous carbon spheres; The chemical composition (wt.%) of the carbon-based bimetallic nanocluster catalyst (PtNCs-RuNCs / PDMC) is: Pt: 2-5wt.%; Ru: 30-35wt.%; C: 55-65wt.%, and the sum of N, O and S contents: 3-5wt.%.

2. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: The N, O heteroatom-doped mesoporous carbon spheres derived from polyaniline in step 2 are uniform porous carbon-based carriers derived from polyaniline, with uniform pore sizes and high integration.

3. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: The RuCl3.3H2O and H2PtCl6.6H2O involved in step 1 and step 3 contain two metal elements, Ru and Pt, respectively.

4. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: In step 1 and step 2, ultrasonic stirring is performed for 30 minutes, and in step 3, stirring is performed for 12 hours.

5. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: In step 5, the temperature of the oil bath is set to 70-90°C.

6. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: In step 6, assemble the reflux pipe and reflux it at 70-90° C. for 1-4 hours to fully reduce the catalyst.

7. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: In the step 7, freeze drying is performed for 5-20 hours.

8. The method for preparing a carbon-based bimetallic nanocluster catalyst according to claim 1, characterized in that: The chemical composition (wt.%) of the carbon-based bimetallic nanocluster catalyst is: Pt: 2-5wt.%; Ru: 30-35wt.%; C: 55-65wt.%, the sum of N, O and S contents: 3-5wt.%; the mass ratios of the porous carbon-based carrier, ruthenium chloride trihydrate, chloroplatinic acid and potassium borohydride during the preparation of the catalyst PtNCs-RuNCs / PDMC are: 43-60: 36-50: 4-10: 135-150.

9. A carbon-based bimetallic nanocluster catalyst according to any one of claims 1 to 8, characterized in that: The carbon-based bimetallic nanocluster catalyst is used for CO2 reduction, wherein the CO2 reduction includes hydrogen evolution reaction and CO2 methanation.