Fluoroferric phosphate material, preparation method and application

By introducing highly electronegative fluoride ions into the cathode material of lithium ion batteries to form fluorinated iron phosphate materials, the problems of low conductivity and insufficient energy density of existing materials are solved, achieving higher conductivity and energy density, and extending the time improved battery life.

CN116281933BActive Publication Date: 2024-10-22UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310011257.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-10-22
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials such as lithium cobalt oxide and lithium iron phosphate have cobalt dissolution problems and low operating voltage, resulting in insufficient life and energy density. New materials need to be developed to improve performance.

Method used

Iron fluorophosphate material is used to embed highly electronegative fluoride ions into the polyanionic structure to form a three-dimensional ion intercalation and extraction pathway, thereby improving the conductivity and energy density, and the material is prepared through plasma technology.

Benefits of technology

It effectively improves the conductivity and energy density of iron fluorophosphate materials, reduces electrochemical polarization, extends the life of the material, and improves the performance of lithium-ion and sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116281933B_ABST
    Figure CN116281933B_ABST
Patent Text Reader

Abstract

The invention discloses a fluorinated iron phosphate material and a preparation method and application thereof. FePO4 is obtained by delithiation of LiFePO4, and then fluorination is performed by plasma enhanced chemical vapor deposition. Compared with non-fluorinated iron phosphate materials, fluoride ions with high electronegativity are selectively introduced into the structure of iron phosphate to construct a fluorinated iron phosphate positive electrode material. Due to the high electronegativity of fluoride ions, a strong P-F bond can be formed, the energy density of the material can be improved, and the diffusion channel of the ions can be widened into a three-dimensional channel, which is beneficial to the transmission of ions, reduces electrochemical polarization, and improves its conductivity. In addition, the introduction of fluoride ions can effectively further stabilize the structure, improve the conductivity, and effectively improve the energy density of the material. The invention has great application prospects in lithium ion and sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a fluoroferric phosphate material and a preparation method and application thereof. Background Art

[0002] The positive electrode material of lithium-ion batteries is one of the most important components of lithium batteries, and largely determines the working voltage, energy density and cycle life of lithium batteries. The current commercial lithium battery positive electrode materials are mainly lithium cobalt oxide and lithium iron phosphate, but they all have their own disadvantages. The problem of cobalt dissolution in lithium cobalt oxide will greatly affect its life, and lithium iron phosphate will reduce its energy density due to its lower working voltage. Therefore, it is necessary to improve its performance or develop a new generation of lithium-ion battery positive electrode materials based on it. Among them, lithium iron phosphate, which is a polyanion positive electrode material, and fluorophosphate positive electrode materials compounded with highly electronegative fluoride ions have the potential to become new lithium-ion battery positive electrode materials.

[0003] However, polyanion cathode materials generally have a series of problems such as low conductivity and large volume changes during electrochemical reactions. At the same time, for safety and cost considerations, polyanion phosphate fluorinated materials have attracted more attention as alternative cathode materials for lithium-ion batteries. Fluorinated phosphate materials embed fluoride ions with high electronegativity into the structure of polyanion cathode materials, making the ion insertion and extraction pathway three-dimensional, thereby improving its conductivity. The introduction of fluoride ions can effectively further stabilize the structure and effectively improve the energy density of the material. Summary of the invention

[0004] In view of the above problems or shortcomings, in order to solve the problem that polyanion positive electrode materials generally have low conductivity, the present invention provides a preparation method and application of a fluoroferric phosphate material. The fluoroferric phosphate material has a special structure and a high transition metal redox potential, and can be used as a positive electrode material for lithium ion and sodium ion batteries.

[0005] To achieve the above-mentioned purpose of the invention, the technical solution of the present invention is as follows:

[0006] A method for preparing a fluoroferric phosphate material comprises the following steps:

[0007] Step 1, preparing an acidic or neutral inorganic salt water solution into a lithium-removing electrolyte with a concentration of 0.01-5.0 mol / L;

[0008] Step 2, using the LiFePO4 electrode sheet as the positive electrode, setting the lithium removal voltage of the LiFePO4 electrode sheet to 0-5 V, not 0, and the lithium removal specific capacity to 170 mAh / g, and performing lithium removal with the lithium removal electrolyte prepared in step 1 and the negative electrode;

[0009] Step 3, washing and drying the positive electrode sheet after electrochemical delithiation in the electrolyte solution in step 2, to obtain the iron phosphate material;

[0010] Step 4: Place the iron phosphate material obtained in step 3 into a crucible in the quartz tube of the plasma tube furnace system, and then use a pump group to evacuate the quartz tube to a vacuum degree of <8×10 -3 Pa, then the tube furnace is heated to 100-600 °C; after the system temperature is stabilized, high-purity CF4 gas with a purity greater than 99.999% is introduced, and then the plasma generating device is started and stopped after a specified operation time of 0-24 hours; after the system temperature drops to room temperature, the product is taken out to obtain a fluoroferric phosphate positive electrode material.

[0011] As a preferred embodiment, the solute of the acidic inorganic salt water solution is selected from one of HCl, H3PO4 and H2SO4.

[0012] As a preferred embodiment, the solute of the neutral inorganic salt water solution is selected from one of LiCl, NaCl, KCl, CaCl2, Na2SO4, and Li2SO4.

[0013] The present invention also provides a fluoroferric phosphate material obtained by the preparation method.

[0014] The present invention also provides an application of the fluoroferric phosphate material in preparing positive electrode materials for primary batteries and sodium and potassium secondary batteries.

[0015] The beneficial effects of the present invention are as follows: compared with non-fluorinated iron phosphate materials, fluoride ions with high electronegativity are introduced into the structure of iron phosphate to construct a fluorinated iron phosphate material. Due to the high electronegativity of fluoride ions, strong PF bonds can be formed, the energy density of the material can be improved, and the diffusion channels of ions can be widened into three-dimensional channels, which is beneficial to the transmission of ions, reduces electrochemical polarization, and improves its conductivity. In addition, the introduction of fluoride ions can effectively further stabilize the structure and effectively improve the energy density of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a schematic diagram of the performance of a primary battery equipped with fluoroferric phosphate material in Example 2 at a rate of 0.1C.

[0017] Figure 2 Schematic diagram of the performance of a primary battery equipped with non-fluorinated iron phosphate material at a rate of 0.1C in the comparative example. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0019] The embodiment provides a method for preparing a fluoroferric phosphate material, comprising the following steps:

[0020] Step 1, preparing an acidic or neutral inorganic salt water solution into a lithium-removing electrolyte with a concentration of 0.01-5.0 mol / L;

[0021] Step 2, using the LiFePO4 electrode sheet as the positive electrode, setting the lithium removal voltage of the LiFePO4 electrode sheet to 0-5 V, not 0, and the lithium removal specific capacity to 170 mAh / g, and performing lithium removal with the lithium removal electrolyte prepared in step 1 and the negative electrode;

[0022] Step 3, washing and drying the positive electrode sheet after electrochemical delithiation in the electrolyte solution in step 2, to obtain the iron phosphate material;

[0023] Step 4: Place the iron phosphate material obtained in step 3 into a crucible in the quartz tube of the plasma tube furnace system, and then use a pump group to evacuate the quartz tube to a vacuum degree of <8×10 -3 Pa, then the tube furnace is heated to 100-600 °C; after the system temperature is stabilized, high-purity CF4 gas with a purity greater than 99.999% is introduced, and then the plasma generating device is started and stopped after a specified operation time of 0-24 hours; after the system temperature drops to room temperature, the product is taken out to obtain a fluoroferric phosphate material.

[0024] In some embodiments, the solute of the acidic inorganic salt water solution is selected from HCl, H3PO4, and H2SO4.

[0025] In some embodiments, the solute of the neutral inorganic salt water solution is selected from one of LiCl, NaCl, KCl, CaCl2, Na2SO4, and Li2SO4.

[0026] The fluoroferric phosphate material is obtained by the above preparation method.

[0027] The fluoroferric phosphate material can be used to prepare positive electrode materials for primary batteries and sodium and potassium secondary batteries. Example 1

[0028] Step 1, preparing H2SO4 into a lithium-removing electrolyte with a concentration of 0.01 mol / L;

[0029] Step 2: Cut the electrode sheet into 4*5cm size, use the LiFePO4 electrode sheet as the positive electrode and the titanium sheet as the negative electrode, set the delithiation voltage of the LiFePO4 electrode sheet to 1.5V, the delithiation specific capacity to 170 mAh / g, and delithiation in an electrolytic cell filled with electrolyte.

[0030] Preparation of electrode sheet: LiFePO4 / C positive electrode active material, conductive agent Super P and binder polyvinylidene fluoride (PVDF) are mixed in a ratio of 90:5:5, and the mixture is prepared into a slurry with 1-methyl-2-pyrrolidone (NMP), evenly coated on the current collector aluminum foil as a positive electrode sheet, and dried.

[0031] Step 3, washing and drying the positive electrode sheet after electrochemical delithiation in the electrolyte solution in step 2, to obtain the iron phosphate material;

[0032] Step 4: Place the iron phosphate material obtained in step 3 into a crucible in the quartz tube of the plasma tube furnace system, and then use a pump group to evacuate the quartz tube to a vacuum degree of <8×10 -3 Pa, then the tube furnace is heated to 100°C; after the system temperature is stabilized, high-purity CF4 gas with a purity greater than 99.999% is introduced, and then the plasma generating device is started and stopped after running for a specified time of 2 hours; after the system temperature drops to room temperature, the product is taken out to obtain a fluoroferric phosphate material. Example 2

[0033] Step 1, preparing Na2SO4 into a lithium-removing electrolyte with a concentration of 0.1 mol / L;

[0034] Step 2: Cut the electrode sheet into 4*5cm size, use the LiFePO4 electrode sheet as the positive electrode and the titanium sheet as the negative electrode, set the delithiation voltage of the LiFePO4 electrode sheet to 2.0V, the delithiation specific capacity to 170 mAh / g, and delithiation in an electrolytic cell filled with electrolyte.

[0035] Preparation of electrode sheet: LiFePO4 / C positive electrode active material, conductive agent Super P and binder polyvinylidene fluoride (PVDF) are mixed in a ratio of 90:5:5, and the mixture is prepared into a slurry with 1-methyl-2-pyrrolidone (NMP), evenly coated on the current collector aluminum foil as a positive electrode sheet, and dried.

[0036] Step 3, washing and drying the positive electrode sheet after electrochemical delithiation in the electrolyte solution in step 2, to obtain the iron phosphate material;

[0037] Step 4: Place the ferric phosphate material obtained in step 3 into a crucible in the quartz tube of the plasma tube furnace system, and then use a pump group to evacuate the quartz tube to a vacuum degree of <8×10 -3 Pa, then the tube furnace is heated to 300°C; after the system temperature stabilizes, high-purity CF4 gas with a purity greater than 99.999% is introduced (the gas flow rate is regulated by a high-precision flowmeter), and then the plasma generator is started and stopped after running for a specified time of 6 hours. After the system temperature drops to room temperature, the product is taken out to obtain a fluoroferric phosphate material. Example 3

[0038] Step 1, preparing Li2SO4 into a lithium-removing electrolyte with a concentration of 5.0 mol / L;

[0039] Step 2: Cut the electrode sheet into 4*5cm size, use the LiFePO4 electrode sheet as the positive electrode and the titanium sheet as the negative electrode, set the delithiation voltage of the LiFePO4 electrode sheet to 5V, the delithiation specific capacity to 170 mAh / g, and delithiation in an electrolytic cell filled with electrolyte.

[0040] Preparation of electrode sheet: LiFePO4 / C positive electrode active material, conductive agent Super P and binder polyvinylidene fluoride (PVDF) are mixed in a ratio of 90:5:5, and the mixture is prepared into a slurry with 1-methyl-2-pyrrolidone (NMP), evenly coated on the current collector aluminum foil as a positive electrode sheet, and dried.

[0041] Step 3, washing and drying the positive electrode sheet after electrochemical delithiation in the electrolyte solution in step 2, to obtain the iron phosphate material;

[0042] Step 4: Place the ferric phosphate material obtained in step 3 into a crucible in the quartz tube of the plasma tube furnace system, and then use a pump group to evacuate the quartz tube to a vacuum degree of <8×10 -3 Pa, then the tube furnace is heated to 600°C; after the system temperature stabilizes, high-purity CF4 gas with a purity greater than 99.999% is introduced (the gas flow rate is regulated by a high-precision flowmeter), and then the plasma generator is started and stopped after running for a specified time of 24 hours. After the system temperature drops to room temperature, the product is taken out to obtain a fluoroferric phosphate material. Comparative Example

[0043] Step 1, preparing Na2SO4 into a lithium-removing electrolyte with a concentration of 0.1 mol / L;

[0044] Step 2: Cut the electrode sheet into 4*5cm size, use the LiFePO4 electrode sheet as the positive electrode and the titanium sheet as the negative electrode, set the delithiation voltage of the LiFePO4 electrode sheet to 2.0V, the delithiation specific capacity to 170 mAh / g, and delithiation in an electrolytic cell filled with electrolyte.

[0045] Preparation of electrode sheet: LiFePO4 / C positive electrode active material, conductive agent Super P and binder polyvinylidene fluoride (PVDF) are mixed in a ratio of 90:5:5, and the mixture is prepared into a slurry with 1-methyl-2-pyrrolidone (NMP), evenly coated on the current collector aluminum foil as a positive electrode sheet, and dried.

[0046] Step 3: Clean and dry the positive electrode sheet that has been electrochemically delithiated in the electrolyte solution in step 2 to obtain the iron phosphate material. (The fluorination step is not performed)

[0047] Battery assembly and testing:

[0048] The two positive electrode sheets of Example 2 and the comparative example were dried and punched into discs with a diameter of 14 mm and placed in the positive electrode shell. An electrolyte solution of 1 mol / L lithium hexafluorophosphate (LiPF6) dissolved in ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3:7 (volume ratio) was added dropwise, and a Cellgard 2400 polypropylene film was placed as a separator. The electrolyte was added dropwise again, and then the metal lithium sheet, gasket, spring and negative electrode shell were placed in sequence. The CR2025 button battery was packaged with a battery packaging machine, and after standing for 12 h, it was discharged at a constant current of 0.1 C to a cut-off voltage of 1.5 V in a constant temperature test room at 25°C for testing.

[0049] The experimental data of the above-mentioned Example 2 and the experimental data of the comparative example are recorded as follows: Figure 1 and Figure 2 As shown, the discharge platform of the discharge curve of the fluorinated iron phosphate material is different from that of the iron phosphate material. From the discharge capacity, it can be seen that the discharge capacity of the fluorinated iron phosphate electrode is higher than that of the comparative example. This shows that the fluorinated material of the present invention can well improve the discharge specific capacity and be applied to lithium ion batteries.

Claims

1. A method for preparing a fluoroferric phosphate material, characterized in that The following steps are involved: Step 1, preparing an acidic or neutral inorganic salt water solution into a lithium-removing electrolyte with a concentration of 0.01-5.0 mol / L; Step 2: Using the LiFePO4 electrode sheet as the positive electrode, setting the delithiation voltage of the LiFePO4 electrode sheet to 1.5-5 V, the delithiation specific capacity to 170 mAh / g, and performing delithiation with the delithiation electrolyte prepared in step 1 and the negative electrode; Step 3, washing and drying the positive electrode sheet after electrochemical delithiation in the electrolyte solution in step 2, to obtain the iron phosphate material; Step 4: Place the iron phosphate material obtained in step 3 into a crucible in the quartz tube of the plasma tube furnace system, and then use a pump group to evacuate the quartz tube to a vacuum degree of <8×10 -3 Pa, then heat the tube furnace to 100-600 °C; after the system temperature stabilizes, introduce high-purity CF4 gas with a purity greater than 99.999%, and then start the plasma generator, running for a specified time of 2-24 hours before stopping; After the system temperature drops to room temperature, the product is taken out to obtain a fluoroferric phosphate positive electrode material.

2. The method for preparing a fluoroferric phosphate material according to claim 1, characterized in that: The solute of the acidic aqueous solution is selected from one of HCl, H3PO4, and H2SO4.

3. The method for preparing a fluoroferric phosphate material according to claim 1, characterized in that: The solute of the neutral inorganic salt water solution is selected from one of LiCl, NaCl, KCl, CaCl2, Na2SO4, and Li2SO4.

4. The fluoroferric phosphate material obtained by the preparation method according to any one of claims 1 to 3.

5. Use of the fluoroferric phosphate material according to claim 4 in the preparation of positive electrode materials for primary batteries and sodium and potassium secondary batteries.